Percy, Metallurgy of Copper and Brass (1861) and of Lead (1870): cementation brass, cupellation, copper roasting and shaft furnaces
Covers period texts read as archive.org OCR text. Page numbers are printed folios read from the OCR running heads; OCR is rough and a few figures are marked as uncertain where a digit or fraction did not survive.
- J. Percy, Metallurgy: Fuel, Fire-Clays, Copper, Zinc, Brass, etc. (London, 1861), archive.org
metallurgyartofe00percrich. Cementation brass pp. 612-617 (the direct-fusion rows of pp. 618-622 are not repeated here); copper blast furnaces pp. 386-411 (Sikkim, Singhana, Japan, Atvidaberg in Sweden), Mansfeld pp. 413-418, Perm pp. 433-435, kernel roasting at Agordo pp. 439-446. Works seen 1848-1861. The Welsh reverberatory process (pp. 314-380) is named only for contrast. - J. Percy, The Metallurgy of Lead, including Desilverization and Cupellation (London, 1870), archive.org
metallurgyleadi00percgoog(Google scan; alsoindia.history.resource.77332, whose text and PDF layer fill pages 180-181 and 183 that the first scan's OCR garbles). English cupellation pp. 177-185, German cupellation pp. 185-208 (Freiberg 186-198, Tarnowitz with coal 204-208), refining of Blicksilber pp. 209-212, lead ore-hearth pp. 279-289. Works seen 1832-1869. - Not found or not used: Ure's Dictionary art. Brass (already digested in the retort file), J. Day, Bristol Brass (no text searched), Agricola (cited by Percy, not read), Rivot. Purpose period facts for the brass wind furnace, the cupellation hearth, the roasting heap and stall, and the copper shaft furnace. INFERRED marks my own reading.
A. Cementation brass furnace (calamine brass)
Place and date
- "Until a comparatively recent period all brass was made by the old process of cementation ... This ancient process, which had been practised for centuries, was, nevertheless, patented in this country in 1779, by Mr. John Champion, senior" (Percy Metallurgy, p. 612).
- Percy saw it "only a few years ago" at Pemberton's works, Birmingham ("the last which survived in that town"), now pulled down; in 1859 "several of these furnaces" still stood at Sims, Nevill and Co., Llanelly, Glamorgan, "and there are others, I am informed, at Swansea" (p. 612). Measurements and process come from Llanelly, via Joseph Stringer, who superintended the furnaces (p. 612).
- History: calamine brass works in Surrey about the middle of the 17th century (Demetrius, a German), Bristol about 1702, Cheadle, Staffordshire about 1720 (pp. 527-528). Calamine brass ceased at Birmingham "because its price was sensibly higher than that of common brass" (p. 618).
Furnace form
- "It exactly resembles ... the furnaces represented in the engravings contained in old metallurgical treatises. It consists of a circular chamber, lined with fire-brick; it is contracted above to a circular opening, the mouth, in which is fixed a cast-iron collar; it is closed at the bottom by a circular cast-iron plate or bed-plate, in which are 12 holes symmetrically arranged round one larger hole in the centre, through which the ashes and clinkers may be withdrawn" (p. 613).
- Below the bed-plate an ash pit with "an arched air-way" to "a long arched passage or vault ... through which air is conveyed to the furnace from the outside" (p. 613). So the draught is natural, drawn in by an underground air passage; "the furnace has no chimney, except the mouth, which is kept more or less closed ... by a circular cover of cast-iron, or of fire-brick set in an iron frame" (p. 614).
- Over the 12 small holes sit "short nozzles or twyers of cast-iron, tapering upwards"; the central hole has none. Nozzles "6 inches high, 2-? inches in diameter at the bottom [OCR; a fraction lost], and 1 inch at the top, inside measure, and 3/8 inch [OCR] in thickness" (about 150 mm high, 25 mm top bore). "The space between the nozzles is filled up level with bricks and fire-clay, so as to form a solid bed 6 inches thick. The air which sustains combustion enters through these nozzles, which are used as a substitute for bars" (p. 614).
- Enclosed "in a solid mass of brick-work"; an iron bar over the air-way arch and in front of the bed-plate carries the load (p. 614). "Several of these furnaces are constructed in a row, and over the whole is built a room of brick covered in with a large brick cone, open at the top, exactly like an ordinary glass-house" (p. 614).
- The chamber is drawn widening "to the height of 13 inches above the upper surface of the bed-plate"; the man who built it said it did not widen; Percy could not settle it (p. 614). Chamber diameter at Llanelly is not given in the text read.
- Pemberton's furnace (Birmingham): "diameter ... 3 feet 6 inches at the bottom, and the height 3 feet 6 inches to the collar" (about 1.07 m); 9 crucibles per furnace, Stourbridge clay, 12 in deep and 8.5 in across (p. 616).
Crucibles
- Llanelly: fire-clay, circular, "12 1/2 in. deep, 8 1/2 in. wide at the top, and 6 1/2 in. in the middle, inside measure; 1 in. thick at the top, and 2 in. thick at the bottom" (about 318 x 216 x 165 mm); holds 84 lb of metal (38 kg) (p. 614; fractions read from OCR "12 J", "81", "6}").
- The "king-pot" in the centre of the bed-plate: 13.5 in deep, 8.5 in wide at the top, 7.75 in at the middle (OCR), 1.25 in thick at the top, 2 in at the bottom; holds 120 lb (54 kg). Another brass-maker says the size difference is unnecessary (p. 614).
- Number: 12 side pots round 1 king pot is INFERRED from the 12 nozzle holes round one centre hole (Fig. 152 is referred to as showing the arrangement; the count of pots is not stated in words at Llanelly). Pemberton: 9 pots.
- Pot life: "good pots lasted on an average 16 days, not being allowed to cool during that period" (p. 615).
- Lid: "covered" only; the cover's material and any luting are not stated (p. 615).
Charge, per pot, and fuel
- "Calcined calamine or blende calcined sweet and ground fine, 100 lbs., ground coal 40 lbs." (not charcoal in this text); dry-mixed, sieved (8 holes to the linear inch), wetted with 2 gallons of water, left half an hour, mixed and sieved again (4 holes), "levelled and thoroughly mixed with 6? lbs. of lean-shot copper" [OCR "6$"; INFERRED about 65 lb from Pemberton's 64 lb copper to 88 lb calamine]. "The mixture should be sufficiently moist to adhere together by pressure with the hand ... produces brass for the best battery purposes, i.e. brass intended for hammering" (p. 614).
- Pemberton, in later times, two qualities, "B. I." and "B. XX.": 64 and 61 lb feathered-shot copper; 88 and 97 lb ground calcined Somerset calamine; 1 bushel coal-slack (p. 616).
- Poorer brass: reduce the copper by 1 lb and add spelter, broken small, in the bottom of the pot (p. 615).
- Fuel: coal. "3 cwt. of coal broken in pieces a little larger than the fist" per firing (about 152 kg) plus four flat coal slabs, "each about 15 in. long, from 3 to 4 in. thick, and 8 or 9 in. wide", laid as a cross over the pots, one end on a side pot and the other on the king pot (p. 615).
- 1781 brass-house account (Forest Works, one week): 1 cwt 20 lb copper shot, 0 cwt 16 lb calamine, bags of charcoal dust, 33 bags of coal; the copper "is estimated to increase 50 per cent. in weight; and the brass, which is composed of 2 parts of copper and 1 of zinc, to be equal to the weight of the calamine used" (p. 616). Charcoal dust therefore appears in the 18th-century works (INFERRED: as the reducing agent), coal-slack in 1859.
Lighting, firing, keeping
- "It is supposed that the furnace has become previously heated in the regular course of working": the furnace is never cold between charges (p. 615). The central hole is stopped with clay before charging (p. 615).
- Pots "charged with care moderately lightly, covered", set on the bed-plate; coal laid on and the tongs placed in the mouth to break its fall (p. 615).
- "The coal is thus left to burn until 'all the gas is out of it,' which will require about 1 1/2 hour, when the cover is placed over the mouth to within 1/2 in. on one side in order 'to harden the coke' formed. After this, the coked coal is cautiously poked down amongst the pots, care being taken to keep the draught holes open and clear. The cover is now placed to within 1 1/2 in. on one side of the mouth, and the furnace may then be left during 3 hours without a further supply of coal. It is the duty of the foreman to see that the draught holes are properly cleared and the pots kept covered with coke. The heat is gradually raised in the course of the process by removing the cover a little on one side" (p. 615). Draught control is the mouth cover and the clearing of the nozzles.
- Heat length: "The process, if properly attended to, will be completed in about 10 hours" (p. 615). Temperature not stated in degrees. The chemistry: zinc oxide is reduced "at a temperature below the melting-point of copper, which, being thus exposed to the action of the vapour of zinc, becomes permeated with this metal"; the temperature must be held so "that the copper shall not melt, but remain diffused through the mass of the charge; for if it were allowed to melt, it would trickle down to the bottom of the pot ... and much of the zinc would then escape" (p. 617).
- Coin experiment: zinc at the bottom of a clay crucible, coarse burnt fire-clay over it, a copper coin in charcoal powder, luted cover, "a gentle red-heat": the coin takes a yellow brass skin keeping its effigy (p. 617).
Collecting the brass
- King-pot out first, stirred with an iron bar with a flat or paddle end; one side-pot out and treated likewise, "the brass, which has subsided to the bottom, is poured into the king-pot"; the rest in turn; the king-pot is shaken during the pouring; the metal is "skimmed and poured into iron ingot moulds". "As soon as a side-pot has been deprived of its brass, it should be replaced while hot in the furnace" (p. 615). The pots are lifted out through the mouth; the lifting tool is not named.
- The king-pot must be the cleanest, with little matter on its sides; the paddle is pushed round the sides, and "by gently bumping the bottoms of the pots on the floor, the subsidence of the metal is promoted" (p. 615).
Yield, cost, crew
- Output per pot or per firing in pounds of brass is not stated for 1859. 1784 account: 14 cwt 2 qr 26 lb copper shot and 22 cwt 0 qr 11 lb calamine gave 22 cwt 0 qr 11 lb of brass, wages 1 pound 4 shillings, "the furnaces in one week" (p. 617). 1781: 14 cwt 0 qr 16 lb of brass (p. 616).
- Crew: "the incessant care which a calamine brass furnace requires, as it is kept in operation during long periods without intermission"; an old furnace-man of 60 years "had scarcely had one continuous night's rest out of five nights every week" (p. 615 note). 1781 wages: two brothers and a helper (p. 616). Number per furnace at Llanelly: not stated.
- Repair between campaigns: furnaces are not cooled; pots are swapped hot. The bed-plate, nozzles and lining repair are not described. Not documented.
- Losses / what goes wrong: copper melting and running to the pot bottom loses zinc (above); a dirty king-pot hinders pouring; badly sealed or over-hot pots lose zinc. A numeric zinc loss for cementation is not given.
B. Cupellation (silver from work lead, litharge)
B1. English cupellation, the test furnace (Llanelly Lead Works, 1859)
- Place and date: "the cupelling-furnaces in operation at the Llanelly Lead Works in 1859" (OCR of the first scan reads 1858), drawings by Mr. Bowen, from Messrs. Nevill (Percy Lead, p. 178). Principle: lead is oxidised by air, litharge flows off, silver stays; Percy's blowpipe-and-bone-ash-capsule illustration, pp. 177-178.
- Why a bone-ash bottom: "there is no better material than bone-ash for a test-bottom, not ... because it is absorbent, but solely because it resists satisfactorily the corrosive action of molten litharge"; on the large scale absorption of all the litharge is impossible ("so thick as to make it very difficult, if not impossible, to keep it hot enough throughout") (p. 178).
- Furnace form: a reverberatory with a large fire-place "compared with the body of the furnace, which is short"; fire- bridge wall and flue-wall with iron doors at front and back; wrought-iron bars carry an oval "compass-ring" of wrought iron in two parts, its upper face covered with brickwork plastered with fire-clay, which surrounds the ring's inner edge except at the front (pp. 178-179). A downward flue leads by two openings to a "high stack by a long underground culvert"; the fume passes a condensing chamber, with a steam jet in the flue (pp. 179-180). The roof is the fixed part; the test is the movable part ("in the German furnace the bed is fixed and the roof moveable, whereas the reverse is the case in the English furnace", p. 185).
- Back and front are cast-iron plates; the back has openings through which "pigs of lead are inserted, and gradually pushed forwards as they melt away, thus providing a continuous supply of fresh lead to the test"; the front has a fire-door, a door beside the test breast where litharge flows over, and a "skimming-bar" of wrought iron as fulcrum for tools (pp. 179-180).
- The test: "a frame of wrought-iron, filled in with bone-ash ... an elliptical ring, made of a flat wrought-iron bar, 4 1/2 in. wide [OCR '4-J-'] and [thickness lost] thick, having a bottom formed of four transverse bars of the same sized iron, placed flatwise ... the ends of these bars are turned up at right angles and rivetted to the ring"; two 2.5 in strap-bars sometimes added (p. 181; "the use of strap-bars is exceptional", p. 182).
- Bottom: bones "calcined to whiteness, pounded, passed through a sieve of 26 holes to the linear inch, and tempered or moistened with water containing pearl-ash dissolved to the extent of 2 1/2 % [OCR '2^%'] of the prepared bone-ash. There should be just enough water to make the mass cohere slightly when squeezed in the hand", "rammed evenly and solidly into the test-frame by means of an iron rammer, such as moulders use" (p. 181). A cavity is scooped with a trowel; the bottom slopes about 1/2 in. (OCR) to a point where a hole can be drilled to drain every particle of metal (p. 182). Bone-ash needed: "about 2 1/2 cwts. [OCR '24'] of dry bone-ash", holding "about 8300 ozs. of silver" (p. 182). Overall test outside size is not legible; a Newcastle (Pattinson) test is "4' long, 2' 6" broad, and 4" deep, outside measure, and containing about 1 1/2 cwt. of bone-ash" (p. 184), about 1.2 x 0.76 x 0.10 m.
- Breast: 13 in (OCR, a fraction may be lost) of bone-ash between the cavity end and the ring, "the breast of the test". A channel "about 2 in. wide at the inner end, 1 in. at the other, and 1/4 in. [OCR] deep" is cut across it to a hole through the end, so litharge "flow[s] over the breast and thence downwards into a cast-iron pot placed underneath"; "there is no contact between the litharge and the iron of the ring" (p. 182). The groove corrodes and is stopped with "a plug of tempered bone-ash"; a second and a third groove are cut in turn; then the test is spent or full of silver (p. 182). A wide breast lets 5 or 6 channels be cut one after another; an 8 in breast also served (p. 185).
- Drying and setting: the new test is "left slowly and completely to dry before use" (p. 182). It is brought up "close against the under side of the compass-ring", luted at the border with paste of the same bone-ash, held by four iron wedges (p. 183).
- Blast: "produced by a steam-jet [i.e. at these works, but it is usually produced by a fan]", a 3/4 in (OCR) steam pipe from a steam-chest at 26 lb per square inch, nozzle reduced to 1/2 in (OCR), into an iron blast pipe 1 3/4 in (OCR) bore, 1/8 in thick; aimed to strike "the middle of the second cross-bar" (p. 182). The ordinary blower is a fan; no bellows kind is named for the English furnace.
- Lighting and run: "the fire is lighted, and the heat very gradually raised to bright redness - say, to a temperature above the melting-point of litharge, but considerably below that of silver - when molten lead is introduced sufficient nearly to fill the cavity. The lead is added molten in order to save time and not to cool the test ... there should be a suitable cast-iron melting-pot attached to the furnace. As soon as the temperature has risen to the melting-point of litharge the blast is let on" (p. 183).
- Litharge: blown to the breast, drops into the pot, which is wheeled away when full and replaced; "when the litharge in a pot is solidified, it is turned out in a cake; and as it cools it swells up, exfoliates, and falls to pieces" (p. 183). Pigs pushed forward through the back openings to keep the test supplied.
- Enrichment: run "until the lead in the test has become enriched, say from 200 to 250 ozs. of silver in the ton to 3000 ozs. in the ton, when it is tapped out into the large cast-iron pot ... by drilling a hole in the bottom of the test ... and cast into pigs"; the hole is replugged with test material and the run resumed; "a test may be thus tapped about once every 24 hours" (pp. 183-184).
- Refining: the enriched lead goes on a fresh test, "not more than 25 tons should be worked off" on one (p. 184). "Towards the completion of the process the fire should be strongly urged, and the silver on no account be allowed to solidify until every trace of lead has been removed"; its litharge, richer in silver, is kept apart. "From 2 to 6 hours elapse, during which the silver gradually becomes fine." On the large scale the sudden brightening "does not occur" (p. 184). The cooling cake "is suddenly thrown up at various points, with the formation of little volcano-like craters, some even several inches in height, through which oxygen escapes"; the surface is pricked to let gas out (p. 184). Cake of silver 5000 to 7000 oz (about 155 to 218 kg troy) is taken out when cold, detached, cleaned, sold or cut up, remelted, and cast in open-topped iron ingot moulds oiled and dusted with charcoal powder (p. 184).
- Fuel and throughput: "About 10 cwts. of coal at Llanelly were required to refine 1 ton of lead" (p. 184). Pattinson: "4 fodders of lead (1 fodder = 21 cwts. = 2352 lbs.) may be converted into litharge in from 16 to 18 hours on a test 4' long ... and 24 fodders of lead can be very easily oxidized in one furnace by three men in a week, with a consumption of about 3 cwts. of coal per fodder of lead" (p. 184, Nat. Hist. Soc. Northumberland, 1832). Dick: "from 20 to 25 tons of lead may be refined per week, though in some places not more than 12 tons"; "the quantity refined in a given time is determined by the blast rather than by the size of the test" (pp. 184-185).
- Loss: "the loss of lead in cupelling ... by the English method may be usually estimated at about 5%" (p. 185).
- Repair: "the tests become partly saturated with litharge by absorption. They are broken up and the saturated portion is smelted in a slag-hearth or otherwise. Fluor-spar ... is an excellent flux for bone-earth" (p. 185). The bone-ash is burned in an arched brick kiln at the works (p. 182).
- Crew: three men per furnace (Pattinson, p. 184).
B2. German cupellation (Abtreiben), the fixed hearth with a hood - Freiberg, Saxony
- Source: Winkler's 1837 description of wood-fired Freiberg practice, with Plattner (1860) additions (Percy Lead, pp. 186-198). Marl bottoms replaced "lixiviated wood-ashes mixed with a little slaked lime" "not ... until 1815" at Freiberg; first used by Tutschnack at Tajova (Schemnitz) in 1796 (p. 185).
- Principle: "the bed is fixed and the roof moveable"; the roof lifts off by a crane so the cake can be got out and the bed renewed, and it also cools the furnace quickly (pp. 185-186, 194). Formerly wood fuel and no roof at all (p. 185).
- Structure (woodcut key, pp. 187-188): drainage channels and foundation walls; iron cramps; a "great ring-wall" (formerly sandstone in clay, now fire-brick); a slag bottom (lead-furnace slag); a dry-set brick bottom grouted with thin marl; over it "a layer of lime-marl from 6 in. to 7 in. thick up to the top of the great ring-wall ... the uppermost and true working bottom, renewed at every cupellation"; a breast over which the lead products flow, with an iron breast-plate covered with beaten marl as a sloping channel and an iron door that lets down to keep in heat; a charging hole through which lead goes in and gas goes out, with a sheet-iron door to regulate draught; a fire-bridge, a fire-place with grate and ash-pit, "there is no chimney"; twyers in a back wall, "the inner opening or mouth of each twyer is provided with a hanging sheet-iron valve which is raised by the blast, so deflecting the latter upon the surface of the molten lead" (Winkler). Furnace diameter and hearth width are on Fig. 41 (Saxon-foot scale) and not in the text.
- Hood: "made of iron bars, and on the inner surface is studded [with] projecting hook-shaped pieces of flat iron, designed to hold the marl-mortar mixed with tow with which it is plastered over"; lifted off by a crane (pp. 193-194). Fume: "provision must in every case be made for conveying away the lead fume" (p. 187).
- Marl: best is 82% carbonate of lime and 16% clay with a little iron oxide, "dark-blueish colour and strong fatty lustre" (Kersten); Harz works mix 30 cu ft marl with 6.5 cu ft clay-slate (p. 188); Tarnowitz uses dolomite with 16 to 20% fire-clay (pp. 190, 206). Too much clay cracks the bottom and makes it too little absorbent (p. 190). Remove pyrites, straw and wood bits: "the lead follows their track, gets underneath, and heaves up the bottom" (p. 190).
- Bottom making: the marl is stamped or ground fine as casting sand, wetted, left some hours, kneaded to "just cohere into a lump when squeezed in the hand"; spread on the sprinkled brick bottom about 8 in thick at the centre and 9 in at the rim, beaten (hand, then an instrument) to 6 in at the centre and 7 in at the rim, following the curve; "a blow with the fist should strongly indent it (?), but not the pressure of the hand and thumb." A cavity 24 to 30 in wide is cut a little nearer the twyers and fire-place and beaten solid with a flat-faced hammer, to collect the silver (pp. 190-192). Proverb: "the more concave the bed the easier is lithargification and the more difficult brightening" (p. 190). The marl bottom "undergoes no preliminary desiccation" - Winkler says it dries less cracked under its lead (p. 193).
- Charge (Winkler, 1837): "about 100 ctrs. of lead" (1 ctr 114 lb, so about 5 tons; 5 t note) of which 65 to 80 first, the rest later; small hemispherical pigs set convex side down, straw sometimes under them (p. 192-193, note). Plattner 1860: 350 to 370 ctrs (60 kg each, about 21 to 22 t) of lead in one operation, about 130 at the start, rest after litharge begins to flow (pp. 197-198). Ore very rich in silver is cupelled by laying it under the first pigs (p. 198).
- Lighting: ignited charcoal on the central pigs, billets of wood over it, hood dropped and luted with clay at its edge, blast let on, fire made on the grate with billet wood (p. 193). "From 3 to 5 hours elapse before the lead is completely melted down." (p. 193).
- Stages (Winkler, pp. 193-196): (1) Abzug (scum, dross, impure) skimmed off through the litharge channel, about an hour, lead liquated from it goes back. (2) Strong firing; bath of lead gently circulates; Abstrich (impure litharge, pasty) forms, the bath draws back leaving the "Glattrand" (litharge border) that absorbs oxide; a furrow is sawn in the litharge-channel bed as near the fire-place as possible, "occasionally even a third" cut as the first corrodes. Abstrich flows from about 1.5 h after the last Abzug and for about as long; wood billets are burned on it if it will not run. (3) When the stream sticks to the breast, Glatte (clean litharge) begins and heat is reduced; "litharge continues to be produced during from 20 to 22 hours, that is, until ... the 'Blick,' or brightening of the residual silver occurs, which usually takes place 30 or 33 hours after letting on the blast" (p. 195). Fresh lead added two pigs at a time through the Schurloch onto a raised border so they melt and cannot slide down; level kept low so lead does not escape with litharge. Litharge border about 15 in, reduced to 10 in and finally 6 in (p. 195). (4) Final: heat "considerably increased"; litharge film driven off the silver; "dark flowers and clouds" over bright moving silver; the "Blick": "the litharge completely disappears, and the metal becomes motionless. Immediately afterwards the blast is shut off, and water poured upon the fire as well as upon the silver" (p. 196).
- Product: Blicksilber has "a hackly fracture, and contain[s] about 94% of fine silver", remainder lead with copper, nickel, cobalt, arsenic; refining further here would spit and lose silver (p. 196). It is fine-burned in another furnace (section B3). Plattner's batch: Blicksilber 520 to 530 lb (260 to 265 kg) from 350 to 370 ctrs (p. 198).
- Accessory products per 100 ctrs of lead (Winkler): Abzug 2 ctrs at 64% lead, Abstrich 1.5 at 73%, furnace-bottom (Herde) 21.5 at 60%, impure litharge in channel 18 at 85%, plus clean litharge (pp. 197-198). Bottoms are "impregnated with oxide of lead, usually to the depth of 2 in. in the middle and 3 in. toward the side of the fire-place" and are smelted in the ore furnace for 58 to 66% lead (p. 197). Plattner: Abzug 4 to 6 ctrs, no Abstrich with refined lead, litharge 320 to 330 ctrs of which part is red litharge sold as such (0.006 to 0.007% silver), the rest "revived" to lead and Pattinsonised; hearth-bottoms 38 to 40 ctrs at 60% lead (p. 198).
- Losses: "the average loss of lead by cupellation is estimated at about 8%; and when bottoms of ashes were used, it was estimated at about 14%. The loss occurs chiefly through volatilization, and much exceeds what takes place in the English process" (p. 197); Plattner 8%, often 10% (p. 198). Lead sometimes gets under the bottom and lifts it: "it must be immediately tapped off as such an accident is irremediable" (p. 197).
- Fuel: wood, 220 to 280 cu ft per 100 ctrs of lead (Winkler); Plattner 162 to 165 cu ft (pp. 197-198). Coal and gas-generators "tried at Freiberg, but without success" (p. 197).
- Duration: Winkler's total from lighting to Blick is about 30 to 33 hours of blast plus 3 to 5 melt-down; Plattner's single cupellation "lasts about 80 hours" (p. 198; text read as '80 hours' in two scans). Crew: not stated. Blast source at Freiberg: not stated ("the blast" via twyers).
B3. German cupellation with coal - Friedrichshutte, Tarnowitz, Upper Silesia (Teichmann, 1867)
- Same construction; fire-place, fire-bridge and flue of fire-brick, rest common brick; the upper ring-wall's wedge bricks "1' long" are all renewed once a year, 900 to 1000 bricks; "the lower part of the furnace ... is not exposed to injury" (pp. 204-205). One twyer with a semicircular eye; the hood must be higher with coal; a damper sends flue to a chimney during melt-down and to condensation chambers once cupellation starts (p. 205).
- Hearth: dolomite (about 49-51% lime carbonate, 37-38% magnesia carbonate) with 16 to 20% fire-clay, made like marl; capacity "from 23 to 19 cubic feet for respective charges of 165 ctrs. of poor and about 130 of rich lead"; the whole charge added at once, no after-charge, to spare enriched lead a long hot time (p. 206).
- Blast: pipe mouth 1.5 to 2 in, "under a pressure of 1/2 lb. [OCR] per square inch ... about 200 to 260 cubic feet of air ... per minute" (p. 207); the text also says 100 to 120 cu ft a minute should be used. Ingots cast dish-shaped to match the bottom's curve; dried 4 to 5 hours before the melt-down finishes; a gutter depth such "that when the blast is stopped the outflow ceases"; poor cupellation taps enriched lead (about 10% silver) through a hole under the channel (p. 207).
- End: hood lifted, fire-bars pulled out, cinders quenched; "in the course of 5 or 6 hours the bottom may be cool enough to admit of the removal of the cake of silver"; within at most 20 hours the bottom is renewed and the furnace reset (p. 207).
- Cost per cwt of litharge in 1864 about 10 silver groschen (1 shilling English), wages the largest item after the cask (p. 209).
B4. Fine-burning (refining Blicksilber): an open test with blast (Freiberg, Winkler, 1837)
- Percy: "the ancient method is exceedingly simple and has been well described ... by Agricola ... a method which would not be adopted in the present day except under particular circumstances" (p. 209). Why a second step: the large furnace uses too much fuel to finish a small weight of silver (p. 209).
- Apparatus: "a test, which is only a large cupel, and ... double bellows or other machine for producing a constant blast." The test is an iron bowl coated with clay-wash and filled with marl "stamped in so solidly that no impression can be made upon it with the thumb"; a hollow "from 9 in. to 11 in. wide and about 3 in. deep" cut with a curved knife, "leaving a thickness of about 1 1/2 in. at the bottom", brushed with clay-wash, dusted with bone-ash, smoothed with a brass ball (p. 210). Older linings: 2/3 lixiviated wood-ash with 1/3 bone-ash, later sulphate of baryta with bone-ash (p. 210).
- Setting: a flat brick hearth "like that of a smith's forge", the test bedded in a cavity with its rim level with the hearth on old marl and ash; a blast pipe in the twyer wall about 1.5 ft above the hearth; blast "a pressure equal to 4 in. of water", directed some inches short of the hollow's centre (p. 210).
- Run: Blicksilber in angle-free pieces piled high; ignited charcoal before the blast, a sheet-iron hoop round the test filled with charcoal; blast on; "the silver is melted down and is in the usual motion in somewhat less than half an hour"; then moderate the heat (silver volatilises), remove the hoop and charcoal, burn dry thin wood between twyer wall and test, remove falling embers; stir at least every quarter hour with a bent iron rod; "fat spots" (litharge with impurities) drift to the rim and soak into the test; test for fineness by dipping a warmed rod and judging the pear-shaped drop; then fire removed and the cake sprinkled with hot water until solid (soap and water or beer in former times) (pp. 210-211).
- Quantity and time: usual charge 50 marks (the text also says 60 marks, about 25 lb avoirdupois); "from half an hour to 3 hours"; add 2 to 4 lb of lead per 60 marks if needed; fuel in Winkler's day 21.85 cu ft charcoal plus 12.4 cu ft wood [OCR figures uncertain]; the used test holds 30 to 60 loths of silver (1 loth about 1/2 oz) (p. 211). Plattner: low fuel, suits impure Blicksilber, "greater loss of silver through volatilization", harder to run (p. 211).
- Indian method (Ain-i-Akbari, 300 years before 1870): "They dig a hole, and having sprinkled in it a small quantity of the ashes of field cow-dung, they fill it with the ashes of Babool-wood; then they moisten it, and work it up into the shape of a dish or coppel; into this they put the adulterated silver, together with an equal quantity of lead ... surrounding the coppel with coals, blow the fire till the metals are melted; this operation they repeat ... in most instances four times are required. The proofs of the metal being pure are, the brightness thereof, and its beginning to harden on the sides" (pp. 211-212). The coppel becomes litharge ("kehrel").
- Also refined on a movable bone-ash test under a muffle (Harz, Oker, Clausthal mint) (p. 212).
B5. Lead ore hearth (brief)
- A "small rectangular blast-furnace or hearth composed of various parts of cast-iron, set in brickwork", under a flue hood to protect the men from lead vapour and sulphurous acid (p. 279). Early 18th-century Derbyshire practice was the ore-hearth with charcoal or dried wood and bellows moved by a water-wheel; by 1782 almost gone there (p. 279); by 1870 confined to the north of England (p. 279).
- Northumberland (Keld Head) hearth: hearth bottom 1 ft 11 in x 1 ft 9 in x 1 ft deep inside; work-stone 3 ft 2 in x 2 ft; cast-iron back-stone 2 ft 6 in wide, 1 ft 2 in high (p. 281). Fuel: peat or light wood, one peat set above the tuyere at each stirring; ore fed about every 10 minutes while the blast is shut off by a valve; in blast day and night for six days a week; Rossie Works average per hearth "about 7500 lbs." of lead a day, "four men, of whom two only work during a shift," wood about a quarter cord (pp. 287-289). Fuller detail is not taken.
C. Roasting copper ore: the heap and the stall
C1. Heaps
- Atvidaberg, Sweden (Percy 1861; Ahrend 1859, Bredberg 1850): "free, or unwalled pyramidal heaps, from 28 to 30 feet square at the base, and built on level ground. A bed of wood, from 8 to 12 inches thick, is first formed, upon which ore is piled in alternation with layers of small charcoal ... until the heap is raised to the vertical height of from 10 to 12 feet. The sides and top are afterwards covered with a layer of small pieces of ore from 3 to 6 inches thick, and over the whole ore dust is thrown" (p. 401). About 8.5 to 9 m square and 3 to 3.7 m high. Ore in fist-size lumps for one roast, larger lumps allowed for the first of two (p. 401). Small ore washed in a revolving cylinder of thin iron bars, gravel and walnut sizes both used to cover the heaps (p. 395).
- Time and cycles: the first roast of the stall type runs "four to six weeks"; the soft ore "is roasted a second time, which requires three or four weeks"; twice-roasted ore broken to hens'-egg size and "should retain sufficient sulphur to furnish, when smelted, a regulus yielding from 20 to 30 per cent. of copper" (pp. 401). Roasting is irregular: "in some parts the ore is but little changed, in others it is properly roasted, while in others again it may be sintered or even run together" (p. 401). Old fault: ore fused solid at the bottom "required to be blasted with gunpowder" while the top had not changed (p. 402).
- What goes wrong: unroasted zinc blende left in the charge made "skumnas" (a zinc-rich infusible matte layer) on the regulus, thrown away for 50 years, about half the copper lost (p. 402). Prevented by roasting blende-rich ore twice, the second time with more charcoal (p. 402). Zinc oxide forms a white coating on the ore in the roast (p. 401).
- Heap pits at Mansfeld (Kreuzhutte, 1860): copper-schist "roasted in pyramidal heaps containing from 6000 to 21000 ctrs. each; the time required ... varies from six weeks to three months" (p. 416). Some schists "continue to burn of themselves after having been once ignited" (p. 415). Agricola (1556) already described the burning of the Eisleben schist in heaps (p. 415).
- Agordo, Venetia, open pile (old method of kernel-roasting, ore with 1.6-2% copper): 6 m (about 19 ft 8 in) wide at base, 2.5 m (8 ft) at top, long truncated pyramids of about 209 tonnes of ore, laid on a bed excavated 4 ft 4 in and filled with washed residues, divided along its length by four or five inclined beds of ore-dust "to intercept the transverse currents of air", covered with residues 4 3/4 to 6 in deep, lit at the corner cavities with chips; "combustion continues to be propagated through the mass at the expense of the sulphur in the ore ... during eight or ten months", cool one more month; sulphur collects from cavities made in the cover from week 5 or 6, yield 0.2% of the ore (p. 441).
- Indian practice (Singhana, 1831): ore ground, mixed with cow dung into sausage pieces 5 in x 1.5 in, sun-dried, roasted in "circular heaps 4 feet broad and 1 1/2 high. The fire was lighted in the evening, and on the following morning the roasted ore, which had a red colour, was smelted" (p. 391). Sikkim: the crude regulus is pounded, kneaded with cow dung into balls, sun-dried and roasted "in a shallow furnace formed of a ring of slag-cakes placed on edge" (p. 390).
- Japan: ore roasted "in solidly constructed and permanent kilns, in which are holes for the admission of air ... under a shed ... alternate layers of faggots and ore, a bed of faggots being first spread over the bottom, where a vent-hole is made. The smoke is so sulphureous as to suffocate one ... The roasting continues during 10 days" (Japanese description: 30 days) (p. 392).
C2. Stalls (walled kilns, open in front)
- Atvidaberg ore kilns, only two: "from each end and the centre of a vertical wall 50 ft. long and 10 ft. high, proceed at right angles three walls 28 feet long, 10 feet high, and 7 feet thick: two rectangular spaces are thus formed, of which each is enclosed on three sides by walls, while the fourth side or front remains open; the upper projecting angles ... rounded off in front. The ground ... is level and horizontal. On the bottom of the kilns wood is piled to the height of 1 foot, and then the largest pieces of ore to the height of 4 feet. On the top of the ore a layer, 4 inches thick, of small charcoal is spread, upon which ore is again piled to the height of 3 or 4 feet, then a second layer of small charcoal, and lastly ore until the kilns are filled. The whole pile is finally covered in front and on the top with a layer 1 or 2 inches thick of the ore dust or schlich. The wood at the bottom of the kilns may now be lighted. Combustion continues from four to six weeks" (p. 401). Each stall is 28 ft deep by 14-ish ft wide (INFERRED from the 50 ft wall carrying two bays, about 8.5 m deep and about 4 m wide between 2.1 m walls).
- Regulus roast-house, Atvidaberg: "a wall 5 feet high and 3 feet thick" down the middle of the house; against each side 13 walls "11 feet long, and from 2 to 2 1/2 feet thick": "24 compartments, or kilns, 12 on each side, open in front, each of which in the clear is 11 feet long, from 4 to 5 feet broad, and 5 feet high" (3.4 m x 1.2-1.5 m x 1.5 m); floor of ore dust and clay 6 in, so 4 ft 6 in above it (p. 405). Charge: 8 in of wood across the floor, the broken regulus piled on it, "about 100 Swedish cwt. (between 4 and 5 tons)" per kiln. The regulus is roasted 4, 5 or 6 times, "turned over" into the next kiln each time; charcoal added in rising measures per firing: none, 1 1/2, 5, 8, 10, 12 measures for firings 1 to 6, the later ones in layers in the heap; "the entire roasting generally lasts from 7 weeks to 2 months" (pp. 405). Two- to six-fire roasts "as 'dead' or 'sweet' as practicable"; the copper concentrates as 'kernels' inside the pieces (p. 405).
- Mansfeld regulus kilns "three-walled kilns, similar to those at Atvidaberg": after the first roasting the contents are turned over, broken up, and pieces needing it are put aside for a second; "the greater part of the ore is usually roasted twice"; "care must be taken to leave sufficient sulphur in the roasted regulus to prevent the separation of metallic copper in the subsequent fusion" (p. 417). Mansfeld/Eisleben process roasts regulus six times, sometimes washing it with water between roasts to dissolve out copper sulphate (p. 416).
- Styrian kilns at Agordo (1853, Lurzer), stall-type with roof: "a long rectangular enclosure within four walls ... divided into sections, and the bed of each ... four inclined planes, sloping towards the four angles ... forming a low pyramid", gutters, air channels at ground level ending in quarter-sphere vessels that also catch flowing sulphur, wall cavities to collect sulphur; "protected from rain by roofing of planks" (pp. 441-442). Charging: wood at the four angles, gutters covered with flint pebbles, chimneys built in the middle of ore courses separated by cubes of ore with ore-dust and water; alternate layers of large and small ore; "the roasting is completed in five or six months, and about 288 tonnes of ore are treated at a time" (p. 443). Result 13.26% kernels (89% "good", 5.02% copper) and 86.74% ferruginous shells at 0.70%; fuel per tonne ore about 0.8 cu ft cord wood; 7 men, piece-work, breaking by 121 workers to 54 kg a day each; the kiln beat the open pile (pp. 443-444).
- Kernel concentration: lumps of 1-2% copper pyrite, gently roasted with air, give a copper-iron-sulphur nucleus in an iron-oxide shell, separated by "a few gentle blows with a hammer" (p. 439). Agordo from 1692; Swedenborg described it in 1734 (p. 439).
D. Copper shaft furnaces
D1. Smallest forms: Sikkim clay furnace and Singhana (India)
- Sikkim, Mahanuddi valley (undated visit; reported by H. F. Blanford of the Geological Survey of India): the ore is copper pyrites with much arsenical pyrites, pounded with a stone mallet, washed in a small tye by women, only the top third kept (pp. 388-389). Furnace "formed of a sandy clay ... built in a bank about two feet high, and consisted of a shallow square cavity, the bottom of which was slightly concave. The back wall ... was carried up to the height of about eighteen inches, in the form of a truncated pyramid, the top being hollowed out for the purpose of receiving the slags ... The front wall was very low, not more than about six inches above the bed, while the side walls ... about one foot above the furnace- bed" - "well compared to an arm-chair" (p. 389). Bellows: two, one each side, seamless goat-skin bags, a boy squatting at each, nozzle moulded by hand with its end within 3 or 4 in of the bed; charcoal only (pp. 389-390).
- Run: furnace heated with charcoal, "a few handfuls of the washed ore, previously dried and mixed with charcoal" thrown on, fused to a pool of regulus under liquid slag; charcoal raked off, slag sprinkled with water and lifted off in cakes with pincers into the back basin; repeat "until a cake of 'crude metal' weighing eight or ten pounds had accumulated" (p. 390). Crude metal pounded, kneaded with cow dung into balls, sun-dried, roasted in a ring of slag cakes, then refined in the same furnace as at first, giving a 4 or 5 lb cake of copper; "three pounds of 'crude metal' were said to yield one pound of refined copper" (pp. 390-391).
- Singhana (Calcutta report, 1831; lat. 28 N): round hut, floor sand, a hollow 12 to 15 in across and 2 to 3 in deep lined with fine sand then ashes; 3 clay nozzles (two opposite, one between) joined by moist clay into a low wall; above it 3 fire-clay rings "about 15 inches in external diameter, 9 or 10 inches high, and about 3 inches thick", reused daily though "the bottom of the furnace required to be reconstructed daily"; poker holes through the base and one through each nozzle; three goat-skin bellows worked by men, women and children; daily (9 to 10 hours) "3 maunds of charcoal (1 maund = 80 lbs.)", "2 1/2 maunds" of ore-dung pieces and "2 or 3 maunds of iron-slag, which was required as a flux, and was brought from a distance"; four persons per furnace for 10 rupees a month; next morning the copper in the hearth went to a refining vessel with one bellows and was cast in 1-ft clay moulds; the copper was "lilac-coloured and brittle"; slag heaps 30 to 60 ft high, so the practice was long (pp. 391-392).
D2. Perm, Russia: oxide and carbonate ore in a small one-twyer shaft (Choubine, 1842)
- Ore: cupriferous sandstone impregnated with chrysocolla, blue carbonate and malachite (about 2.5% copper), smelted with 30% dolomite, charcoal fuel (p. 433). Blast furnaces "having one twyer each and a fore-hearth like the Atvidaberg furnaces": shaft 14 ft 7 in high, mouth 2 ft diameter, belly 3 ft 6 in by 3 ft 1.5 in, hearth 3 ft 6 in by 2 ft and 2 ft 4 in deep, semi-elliptical fore-hearth 1 ft x 10 in x 13 in deep; 3.7 to 4.5 tons of ore a day; products slag, cupriferous pig-iron (high iron reduced from the charge, 12.6% copper) and black copper, tapped once in 24 hours (p. 433). Black copper about 90% copper (p. 434). The cupriferous pig-iron was then cooked in a refining hearth with charcoal and the iron slagged off, "491 kil. ... of cupriferous pig-iron ... in twelve hours ... 73.5 kil. of black-copper" (p. 435).
- Percy on oxide ore generally (Vivian's 1859 patent): "Ores of copper which do not contain sulphur are also treated in a similar manner, that is to say, by smelting in a blast-furnace; and thus metallic copper is at once obtained from such ores, in place of ... reducing the copper contained in such ores to the state of regulus, by smelting them with regulus containing an excess of sulphur" (p. 387). Blast-furnace smelting is the old method: "In former times all copper was smelted in furnaces of this description" (p. 387).
D3. Atvidaberg ore furnace (Sweden, Bredberg 1844-48, Malmqvist 1861) - roasted sulphide to matte (regulus)
- Place/date: Atvidaberg, near Linkoping, the kingdom's largest copper works (p. 395). Ore chalcopyrite with iron pyrites and silica; Fahlun ore dresses to 4% black copper, Atvidaberg 5% (p. 395).
- Form: "a quadrangular shaft, open above, and below terminating in a shallow cavity called the hearth", a tap-hole channel at one corner; sides and back "walls built up from the ground", the front closed by a wall carried on a tymp-iron, a thin vertical "fore-wall" that can be taken down; a fore-hearth open above in front, with a hood to take away sulphurous gases (p. 396). "The interior of the furnace is built of mica-schist, in which the mica is sometimes replaced by talc." Walls double, the gap filled with sand "so that the inner walls can be removed ... without disturbing the outer walls" (p. 397). Braced with tie-rods and cast-iron plates (p. 397).
- Hearth lining: 4 in of equal sand and clay stamped moist on the bottom, sides coated wetter, dried "by a gentle charcoal fire"; then a second lining of equal measures of clay, sand and charcoal dust; tap hole rammed with clay with a stick 2 to 3 in thick driven to 3 or 4 in of the inside (p. 397).
- Twyers: "nearly horizontal", of bent iron plate 8-9 in wide and 1/? in thick (OCR '1/4'), copper blast pipes 1.25 in bore; "double-acting blowing-cylinders" (p. 397). Bredberg's furnace: 18 ft high, hearth 3 ft 8 in wide by 5 ft 4 in front to back; shaft 3 ft 10 in at the twyers, 4 ft at 8 ft up, 3 ft 6 in at the top; 3 twyers 4 ft above the hearth bottom, 12 in apart (pp. 397-398). Present furnaces (1861): 24 ft high with a 1-ft partition wall from 10 ft up "for a more even descent of the charges, adopted when coke was first used"; 6 ft wide at the top, twyers 4 ft above the hearth (p. 398). Hot blast from waste gas tried 1861 (p. 398).
- Charge: roasted ore mixed with black-copper slags (rich in iron protoxide), with lime carbonate as flux if needed; "the proportions ... are so adjusted, that a regulus may be formed in which the copper shall not be under 20, nor above 30, per cent.; and a slag, in which the oxygen of the silica shall as nearly as practicable be double that of the bases" (the slag 3 FeO.2 SiO2) (pp. 402-403). Mixed and weighed on a steelyard at each charge, counted on a peg board (p. 403).
- Working: a "nose" or slag prolongation of the twyer 4 to 6 in long; when the "eye" seen through the twyer is dark, poke it clear, and add fuel without ore if the nose grows (p. 403). 60% of the slag runs out clean into a sand bed ("contains from 1/4 to 1/2 per cent. of copper"); the rest crusts in the fore-hearth and is lifted off with a two-pronged fork on a crane and remelted (pp. 403-404). The furnace is tapped only when the hearth is full of regulus, every 48 to 72 hours, 4 to 6 tons a time onto a sand bed, broken fist-size when cold two days later; the blast is shut off to tap by driving an iron bar into the tap-hole, which is stopped with a 6-8 ft wooden stick 2-3 in thick rammed with sand (p. 404).
- Faults: "Eisensau" (bear), iron reduced to a mass in the hearth; with over-roasted ore add raw ore, with sulphur-rich ore it is suppressed; refractory lumps higher up from excess silica, cured with more black-copper slag (p. 403). Zinc vapour forms furnace-calamine crusts, cut out every month to 5 or 6 ft from the mouth; the hearth narrows with stony masses and "after the lapse of from 3 to 4 months" the lower shaft is injured enough to blow out; "the upper part may last several years"; one furnace "may be kept continuously in work during 3 or 4 months" (pp. 397, 404).
- Yield: regulus is "17 to 20 per cent., or even more, of that of the charge", copper in regulus 20 to 22%, 18% in 1859 (p. 404). Slag has about 1/2% copper in all; total loss of copper (the slag) about 1/4% of the raw material by Malmqvist (p. 411).
- Fuel: charcoal formerly, now coke: "1 cwt. of coke is equal to 2 cwt. of charcoal"; "to smelt 4 tons of the materials ... 1 ton of charcoal is required; but 1 ton of a mixture of charcoal and coke will smelt 5 tons" (p. 404). Whole-process fuel per ton of copper in 1858: 240 cu ft pine, 7 tons charcoal and 3.8 tons coke (p. 411).
- Crew: not stated.
D4. Atvidaberg black-copper furnace and refining hearth - matte to copper
- Black-copper furnace "much smaller than the ore-furnace": twyers 10 in apart, inclined 3.5 degrees to the horizon; blast pipe 1.25 in bore, "blast ... at a pressure equal to a column of mercury of 1/2 inch" (OCR); tap-hole feeding a 36 ft iron channel of 10 compartments (p. 399). Enlarged 1859: 17 ft 3 in high, partition wall at 6 ft 6 in, hearth 2 ft 4 in x 2 ft [OCR '24x20'], 3 twyers 2 ft above the hearth; fuel cut 19% and daily yield up 23% (p. 399).
- Charge actual: roasted regulus 200 lb, roasted thin regulus 40 lb, ore-furnace slags 20 lb, cupriferous products 20 lb, quartz 10 to 20 lb (p. 405). Layers in the hearth, bottom up: black copper, thin regulus (55 to 72% copper), slag (p. 406). Slag tapped through the sand-stopped breast; black copper tapped into iron moulds every two or three days; yield 20 to 30%, lately under 20% (p. 406). Black copper 94.4% Cu (analysis, p. 408).
- Refining hearth: "a shallow, generally semicircular cavity ... in a platform of brick or stone-work" lined with clay and charcoal dust or fire-clay and sand; Atvidaberg's is 2 to 2.5 ft across, 15 to 18 in deep, in a platform 16 in above ground topped with iron plates, a copper twyer projecting 4 in, inclined 45 degrees, bore 1.25 in, blast 1.75 to 2.75 in of mercury (pp. 399-400). Charge 13 to 15 cwt of black-copper pigs on charcoal; "the surface of the melted copper must be kept covered with charcoal"; slag skimmed twice or thrice after quenching with water; trial pieces ("Gaarspahn") dipped through the twyer to judge refining (pp. 406-407). Product 99.46% Cu, cast in iron ingot moulds, or lifted off in water-quenched discs (rosette copper) on the Continent (pp. 408-409). Copper "rain" of fine shots up to 4 ft is caught under sheet iron (p. 410).
D5. Mansfeld copper-schist smelting (Prussian Saxony)
- Smelted "at least during several centuries"; Agricola (1556) describes the Eisleben heap burning (p. 415). Schist bed 10 to 20 in thick, of which only 3 to 5 in worth smelting, 2 lb copper per ctr at worst, about 3% (200 lb per Fuder) at Kreuzhutte (pp. 413-416). Silver was long taken out of black copper by liquation with lead; mercury in 1831, then wet methods; by 1861 only one works desilverizes (p. 416).
- Kreuzhutte furnace (1860): "blast-furnaces about 20 feet high"; cylindrical to the hearth top, square hearth section; top diameter 3 ft, 5 ft at 10 ft 6 in down, 5 ft 8 in at 11 ft 6 in, 3 ft 9 in at 14 ft, 2 ft 6 in at the bottom, total 19 ft; two twyers opposite each other, 2 ft 2 in above the bottom, bore 1.5 to 2 in; blast "equal to that of a column of water from 8 to 10 inches in height" (p. 416-417). Matte runs continuously into two conical pits (about 18 in across, 2 ft deep) used alternately - the "Brillenofen" (spectacle furnace) (p. 416).
- Charge: 2 Fuder (about 3 tons English) roasted schist, 8 ctr fluor-spar, 6 ctr concentration slag, plus residues; coke 5 tons measure per Fuder; product ore-furnace regulus (Rohstein) 30-35% copper, slag 0.06-0.15% copper (p. 417).
- Earlier Sangerhausen route (to 1831): roast schist, fuse with slags and fluor-spar to 30-35% regulus, roast regulus in 3 fires, fuse to 50-60% concentrated regulus (Spurstein), roast in 7 fires, fuse to black copper plus rich thin regulus (Dunnstein) 63%, refine, toughen (p. 415).
D6. Welsh process, for contrast only
- Copper in six operations in reverberatories at Hafod, Swansea (1848), roasting in calciners, fusing to coarse metal, white metal, blue metal, then blister and refining (Percy contents and pp. 314-380); a blast furnace was only an adjunct there for slags, in 1859 (Vivian's patent, pp. 386-387). Not read in detail.
E. Dates and places of the practice, collected
- Cementation brass: made "for centuries"; Champion's patent 1779; Surrey works mid-17th c., Bristol 1702, Cheadle 1720 (pp. 527-528, 612); Birmingham till about 1855-58; Llanelly and Swansea in 1859 (p. 612). Direct fusion superseded it (Emerson 1781, see the retort digest).
- Cupellation: Freiberg wood-fired hood furnace to 1837, lime-marl bottoms from 1815 (p. 185); Tarnowitz coal-fired 1867 (pp. 204-209); Llanelly test 1859 (p. 178); Pattinson at Newcastle 1832 (p. 184); Indian cow-dung-ash coppel in Akbar's time, about 1590 (p. 211).
- Copper: Atvidaberg 1844-1861 (p. 395); Mansfeld since "several centuries", Agricola 1556 (p. 415); Agordo kernel roasting since 1692 (p. 439); Perm 1842 (p. 433); Singhana 1831 (p. 391); Japan, Thunberg 1771 (pp. 392-394).
Gaps
- Temperatures in degrees for brass, cupellation or copper smelting: none, only colour terms ("bright redness", "gentle red-heat"). Pyrometric figures are not in these texts.
- Llanelly brass furnace chamber diameter and height, the number of side pots in words, the cover's material, who lifts the pots and with what tool, crew size per furnace, brass yield per firing in 1859, a numeric zinc loss, repair of the bed- plate and nozzles, charcoal quantities (1859 uses coal).
- English cupellation: the test's exact inside size (figure lost in OCR; only the Newcastle test's outside size and the breast and ring-bar numbers), the thickness of the ring bar, the furnace's inside height, the cost of bone-ash by weight per silver weight, a hand-bellows version.
- German cupellation: furnace diameter and hearth width (Saxon-foot scale on Fig. 41), crew, blast machine at Freiberg, blast pressure at Freiberg, the exact silver ounces per batch (given only as lb of Blicksilber), temperature.
- Copper: crew and blast machine at Atvidaberg's ore furnace beyond "double-acting blowing-cylinders"; hearth lining life in days for the small Indian forms; a low sulphide-matte shaft furnace in bellows form for Europe; the yield of copper from oxide ore in the Perm furnace (only black-copper and cupriferous pig-iron are described); first-hand figures for a stall's hours of attention.
- Not reached: Ure art. Brass for cementation, J. Day Bristol Brass, Agricola (Percy cites p. 385-492 of his 1561 edition for refining and p. 218 for heap roasting), Rivot.
Table
| Furnace | Inside size | Draught / blast | Charge | Heat length | Products | Page |
|---|---|---|---|---|---|---|
| Cementation brass furnace (Llanelly 1859) | circular chamber, bed 6 in of brick on cast-iron plate with 12 nozzles; diameter not given; Pemberton: 3 ft 6 in x 3 ft 6 in | natural, air vault to ash pit, cast-iron nozzles 6 in high; mouth cover | 12 pots of 84 lb + king-pot 120 lb: per pot 100 lb calcined calamine, 40 lb ground coal, about 65 lb copper shot; coal 3 cwt per firing | about 10 h per firing; pots kept hot 16 days | brass, 2 Cu : 1 Zn, poured into ingot moulds | Percy Metallurgy 612-617 |
| English cupellation test (Llanelly 1859) | test frame bar 4.5 in; Newcastle test 4 ft x 2 ft 6 in x 4 in outside; breast 13 in; holds 8300 oz Ag | steam jet (or fan), pipe 1.75 in bore | molten lead, pigs pushed through back; 200-250 oz/ton to 3000 oz/ton; refining a further 25 tons per test | tapped about every 24 h; 16-18 h for 4 fodders (Pattinson); refining 2-6 h | litharge into iron pots; silver cake 5000-7000 oz; loss 5% | Percy Lead 178-185 |
| German cupellation hearth with hood (Freiberg) | marl bottom 6-7 in thick, cavity 24-30 in wide; hearth diameter not given | twyers from the back wall, hood lifted by crane; wood on grate | 100 ctr (about 5 t) Winkler; 350-370 ctr (about 21 t) Plattner | melt 3-5 h, litharge 20-22 h, Blick at 30-33 h; Plattner 80 h | litharge, Blicksilber 94% Ag; loss 8% lead | Percy Lead 185-198 |
| German cupellation, coal (Tarnowitz) | bottom 19-23 cu ft; 1 twyer | pipe 1.5-2 in, 1/2 lb/sq in (OCR), 100-260 cu ft/min | 130-165 ctr, whole charge at once | melt 4-5 h; cool 5-6 h; reset within 20 h | litharge, enriched lead 10% Ag or Blicksilber | Percy Lead 204-208 |
| Fine-burning test (Freiberg, open test with blast) | marl hollow 9-11 in wide, 3 in deep, 1.5 in bottom | pipe about 1.5 ft above hearth, 4 in water | 50-60 marks Blicksilber (about 25 lb) | melt under 0.5 h; 0.5 to 3 h | fine silver cake | Percy Lead 209-211 |
| Copper roasting heap (Atvidaberg) | 28-30 ft square base, 10-12 ft high | natural, wood bed 8-12 in, charcoal layers | fist-size ore, ore dust cover | 4-6 weeks first roast, 3-4 weeks second | roasted ore to 20-30% Cu regulus | Percy Metallurgy 401-402 |
| Copper roasting stall (Atvidaberg ore kiln; regulus kiln) | three walls 28 ft x 10 ft x 7 ft thick, open front; regulus kiln 11 ft x 4-5 ft x 5 ft | natural | ore 4 ft + charcoal layers + 3-4 ft; regulus 4-5 t per kiln, wood 8 in, charcoal rising to 12 measures | ore 4-6 weeks; regulus 4-6 fires, 7 weeks to 2 months | roasted ore; roasted regulus | Percy Metallurgy 401, 405 |
| Agordo pile / Styrian kiln | pile 6 m base x 2.5 m top, 209 t; kiln 288 t | natural, ore-dust chimneys, floor channels | cupriferous pyrite 1.6-2% Cu | pile 8-10 months; kiln 5-6 months | kernels 13% (5% Cu), sulphur 0.2-1.1% | Percy Metallurgy 441-444 |
| Sikkim clay furnace | box about 1 ft deep, back wall 18 in, front 6 in, sides 1 ft; bank 2 ft | two goat-skin bellows worked by boys | a few handfuls dried ore + charcoal per round | rounds to 8-10 lb crude metal; refining same furnace | 3 lb crude : 1 lb refined copper (4-5 lb cake) | Percy Metallurgy 389-391 |
| Singhana hut furnace | hearth 12-15 in across, 2-3 in deep; 3 fire-clay rings 15 in OD, 9-10 in high; bottom rebuilt daily | three goat-skin bellows | 240 lb charcoal, 200 lb roasted ore-dung pieces, 160-240 lb iron slag a day | 9-10 h a day | copper next morning; refined in a second small furnace | Percy Metallurgy 391-392 |
| Perm shaft furnace (oxide and carbonate ore) | 14 ft 7 in high, mouth 2 ft, belly 3 ft 6 in x 3 ft 1.5 in, hearth 3 ft 6 in x 2 ft x 2 ft 4 in | one twyer, fore-hearth | 3.7-4.5 t ore a day + 30% dolomite, charcoal | tapped every 24 h | black copper 90% Cu, cupriferous pig-iron, slag | Percy Metallurgy 433-435 |
| Atvidaberg ore furnace (roasted ore to matte) | 18 ft (Bredberg), 24 ft (1861); hearth 3 ft 8 in x 5 ft 4 in | 3 twyers, cylinders, charcoal / coke | roasted ore + black-copper slags, regulus 20-30% Cu | tapped 48-72 h, 4-6 t of regulus a time; campaign 3-4 months | regulus 17-20% of the charge; slag 1/2% Cu | Percy Metallurgy 395-405 |
| Atvidaberg black-copper furnace | 17 ft 3 in high; hearth 2 ft 4 in x 2 ft | 3 twyers, 3.5 degrees down, 1/2 in mercury | 200 lb roasted regulus + 40 + 20 + 20 + 10-20 quartz | tapped every 2-3 days | black copper 20-30% of charge (94% Cu) | Percy Metallurgy 398-399, 405-406 |
| Refining hearth (Atvidaberg) | 2-2.5 ft across, 15-18 in deep | copper twyer 45 degrees, 1.75-2.75 in mercury | 13-15 cwt black-copper pigs | one run, trial pieces every spell | refined copper 99.5% | Percy Metallurgy 399-400, 406-409 |
| Mansfeld (Kreuzhutte) | about 19-20 ft high, top 3 ft, belly 5 ft 8 in, bottom 2 ft 6 in | 2 opposed twyers, 8-10 in of water | 2 Fuder (about 3 t) roasted schist, 8 ctr fluor-spar, 6 ctr slag, coke 5 tons measure | continuous tap | regulus 30-35% Cu; slag 0.06-0.15% Cu | Percy Metallurgy 416-417 |
| Lead ore hearth (Northumberland) | 1 ft 11 in x 1 ft 9 in x 1 ft; work-stone 3 ft 2 in x 2 ft | bellows by water-wheel, peat and wood | ore every 10 minutes | blast day and night, 6 days a week | 7500 lb lead a day per hearth, 4 men | Percy Lead 279-289 |