Covers H. Bessemer, "Sir Henry Bessemer, F.R.S.: An Autobiography" (1905, 504 PDF pages). Pages below are the book's printed folios. The offset between PDF page and folio grows with every plate: 42 at folio 138, 56 from folio 151, 60 at 203, 66 at 207, 70 at 224, 74 at 231, 86 at 257, 88-92 through 281-295, 110 at 337-341. PDF pages 2-6, 8, 10, 18, 22, 35-36, 46, 57-58, 71, 73, 83, 126, 141, 149, 157-158, 186-187, 194, 198, 201-202, 204, 206, 252, 261-262, 265-266, 268, 270, 276-277, 298, 301, 309-314, 328, 335-337, 367, 373, 377, 398, 401, 403, 410, 415, 425-426, 449-452, 454, 457, 460, 467-470, 472, 502 and 504 carry no text layer; those inside the steel chapters are the blank backs of plates. Plates XIII (facing p. 143), XIV (p. 146), XV (p. 148), XVI, XVII and XVIII (p. 150) and Fig. 47 (p. 150) were read from renders; Plate XVIII at 250 dpi in two crops. Read: Ch. XI-XII whole (pp. 138-177: the reverberatory trials, the fixed and tilting converters, the Cheltenham paper of 1856, the licensees' failures, phosphorus); Ch. XIII (pp. 178-188: Bessemer pig, Swedish pig, the Sheffield works); spot pages of Ch. XIV-XVI (pp. 192-194, 203, 207, 224, 231-233); Ch. XVIII whole (pp. 256-295: manganese, Mushet, spiegeleisen, ferromanganese, Swedish and Austrian practice); the American plant in Ch. XXI (pp. 337-341). Skipped: Ch. I-X (stamps, bronze powder, sugar, glass, guns), the gun, plate and Armstrong controversy of Ch. XIV-XVII beyond the spot pages, the saloon steamship (Ch. XX), and the rest of Ch. XXI. The numbers in Ch. XVIII are Bessemer's own and partisan against Mushet; the Hewitt report he quotes (pp. 273-276) and Campbell corroborate them. Subject the converter, its ladle and the steel it made: the blow, the vessel, the gear, the pit, manganese and spiegel.
What the book says
Before the converter (pp. 138-143)
- Steel was blister bar melted in crucibles of at most 60 lb (p. 138). His first route was a reverberatory furnace melting blister steel into a pig bath; hot air through a perforated fire-bridge decarburised the bath (p. 139). Pieces of pig left in that air turned to "thin shells of decarburised iron" (p. 142).
- A crucible with a clay blow-pipe converted 10 lb of grey pig in thirty minutes, but only inside a hot air furnace (p. 143, Fig. 38).
The fixed converters (pp. 143-148, 157-159; Plates XIII, XIV)
- First vessel: a flat-topped cylinder about 4 ft high inside, six horizontal tuyeres round the lower part fed from an annular air chamber, 10-15 lb blast, 7 cwt of pig run in through a hopper (p. 143, Fig. 39).
- The blow as he first saw it: "All went on quietly for about ten minutes; sparks such as are commonly seen when tapping a cupola, accompanied by hot gases"; then "an ever-increasing stream of sparks and a voluminous white flame", "a succession of mild explosions, throwing molten slags and splashes of metal high up into the air"; "in ten minutes more the eruption had ceased, the flame died down, and the process was complete" (pp. 143-144). A cast-iron plate hung over the mouth melted and fell away (p. 144).
- Fewer or smaller tuyeres or a weaker blast "only resulted in a reduction of the necessary temperature"; one such trial left "a solid mass of brittle white iron" after more than an hour (p. 145). "Rapidity of action, ending in a violent eruption, is an absolutely necessary condition of success"; the metal must be "very considerably above the mere melting temperature" so it does not chill in the pour, under a cool addition, or in the ladle while the ingots are cast (p. 145). Large vessels leave 8-10 ft above the bath for the eruption (p. 145).
- Second vessel: an upper chamber with an arched roof and a sloping floor returning splashes, two lateral openings for flame and slag, used also to heat scrap and recarburisers; six fire-clay or plumbago tuyeres rammed in loam, "easy removal when worn out" (p. 146, Figs. 40-41). A hopper and spout from the cupola, a tap-hole and a spout into a shallow pan with a fire-brick plug (pp. 146-147, Fig. 42).
- The Cheltenham paper, 1856: a cylinder 3 ft across and 5 ft high, five fire-clay tuyeres about 2 in above the bottom, a tap-hole stopped with loam; one to five tons a charge; the vessel "so near to the discharge hole of the blast furnace as to allow the iron to flow along a gutter into it"; blast 8-10 lb (p. 157). After relining, a coke fire dries and heats the vessel and is raked out (p. 157). The blast is turned on before the metal runs in, or the metal enters the tuyeres (p. 158).
- The paper's blow: flame "and a few bright sparks" for fifteen or twenty minutes; then "an immense increase in the volume of flame", the metal rising several inches, "a light frothy slag ... thrown out in large foam-like masses" for five or six minutes; then "a steady and powerful flame" for about ten minutes, "when it rapidly falls off. As soon as this diminution of flame is apparent the workman will know that the process is completed" (p. 158). Loss 12.5 % on four experiments, to ingot iron (p. 158). The surplus heat remelts crop ends, runners and scrap piled in the upper chamber "without any loss or expense" (p. 159).
- Too small a set of tuyeres failed to bring on the boil in an hour and three quarters; two thirds of the charge froze. "A fresh charge of fluid iron ran into the vessel, which had the effect of entirely remelting the former charge" (p. 159).
- Stopping: "at a certain period of the process, any quality of metal may be obtained"; semi-steel loses "about 2.5 per cent less" by oxidation than iron (p. 161).
The tilting vessel (pp. 148-151, 192; Plates XV-XVIII, Fig. 47)
- Why tilt: a fixed vessel blows while the metal runs in and while it is tapped, for an uncertain time, and cannot stop if the blast engine fails or a tuyere gives way. On axes the tuyeres stay above the metal while it runs in, the blow starts all at once, stops for the discharge, and "a stoppage of the process" can be made at any time to change a tuyere (p. 148).
- The shape: arched in all directions so the lining holds upside down; "a long oval form" giving "some eight or nine feet in height for the metal to throw itself about in"; "the large mouth or outlet pointing to one side ... so that the sparks could be discharged away from the casting pit" (p. 148). Plate XV draws it: an egg on two cast A-frame standards, a beak-shaped nose off-centre, four poses (A elevation; B on its back for running in, the bath lying in the belly below the tuyeres; C upright blowing, the whole bath a froth; D turned down pouring into the ladle E). G is the bottom: seven round tuyeres, each pierced with several holes; H a tuyere brick in section with its bores. The tuyere bricks run through the bottom into a box beneath (Plate XV, C).
- The tilting gear: shafting and straps are unfit because the load reverses as the metal runs to the nose and "the converter might swing itself round and discharge the incandescent metal on to the floor"; hence hydraulic gear, with which "a lad at a safe distance can start or stop it instantly" (pp. 149-150). The first Sheffield vessel "was moved by hand-gearing" (p. 150): Plate XVI draws a large spur wheel on the trunnion and a pinion on a crank shaft in the standard. Plate XVIII, the later plant in plan: a horizontal hydraulic cylinder along the back wall drives a rack on the pinion of the back trunnion; the blast pipe enters the front trunnion through a valve.
- The other contrivances: a blast engine with self-acting valves; "the hydraulic crane carrying the pouring ladle over every mould in the semi-circular casting pit, and designed to rise and fall in accordance with the movement of the converter"; ingot cranes that clear and refill the pit; "the elevated valve-stand, from which safe position a single workman can overlook the whole converting apparatus, and control all their movements, govern the blast, and work the hydraulic cranes" (p. 149).
- The ladle: "loamed-up", with "a discharge valve at the bottom", moved from mould to mould with the valve shut, pouring "a vertical stream down the centre of the mould" worked by a hand lever. A lip pour curves, strikes the far side of a narrow mould and welds ingot to mould, and carries floating slag into the ingot (pp. 148-149; Plate XV E-F, Plate XVI). The ladle's contents, "well stirred by the revolving agitator", cast ten ingots "absolutely identical in quality" (p. 233).
- The plant (Plates XVII, XVIII): two converters on the flat side of a semicircular sunk pit, each under its own hood and stack; a central slewing ladle crane, ladle at one end of the jib and a counterweight at the other; ten moulds on the arc of the pit; stairs at both ends. Fig. 47: a jib ingot crane with tongs lifting a square ingot. The system of 1858-62 is "the tipping vessel ... with the ladle provided with a bottom valve, the conical mould, and the hydraulic crane" (p. 192). Works ran vessels in pairs: Woolwich (p. 188), Neuberg (p. 276), Troy and Harrisburg (pp. 339-340).
- Holley in America: raised the vessels off the deep pit, top-supported cranes, three ingot cranes, all worked from one point, cupolas in place of reverberatories, and a weighing ladle between cupola and vessel; the vessel bottom's short life was his worst difficulty (p. 341).
The mould (pp. 147, 153, 232)
- The first mould: 10 in square, about 3 ft long, water-jacketed, on a hydraulic ram whose head is the mould's bottom; "an interval of eight or ten minutes" and the ingot, 10 in square and about 7 cwt, rises out standing on end (pp. 147, 153). Later moulds are conical (p. 192). A 10-ton converter casts eleven ingots 1 ft square of 18.5 cwt each, 3 cwt cropped off each top (p. 232).
The blow in the Sheffield works (pp. 152-153, 174, 187, 207, 224, 231)
- Silicon, 1.5-2 % of the pig, burns first: "very undemonstrative, a few sparks and hot gases"; after ten or twelve minutes the carbon, about 3 %, gives "a voluminous white flame ... and brilliantly illuminates the whole space around". The drop "took place almost suddenly" (pp. 152-153).
- Blow times: 15-20 minutes on Swedish pig (p. 174); "In about twenty minutes the flame had dropped, the mouth of the huge vessel was gradually lowered" (p. 187); ten to twenty minutes (p. 224); thirty minutes (pp. 153, 161, 231). "The huge white flame issuing from the converter suddenly drops when all the carbon is burnt out, a result which occurs with unerring certainty" (p. 207).
Phosphorus and the answer (pp. 170-179, 192-194, 289, 293)
- The licensees' fixed vessels at Manchester, Dowlais, Butterley and Govan failed: their pig carried phosphorus (p. 170). His own London trials had used Blaenavon grey pig in a clay or firebrick lining; the licensees lined with siliceous material (p. 171). Hydrogen, gases and fluxes failed to remove it (p. 172).
- Swedish charcoal pig "converting it into pure, soft, malleable iron, and also into steel of various degrees of hardness ... wholly without the use of manganese or spiegeleisen", 15-20 minutes (p. 174). The first large Sheffield ingot, Swedish pig, "no spiegeleisen or manganese in any form" (p. 181).
- Workington's hematite ore was pure but its pig was not: the furnace was fluxed with puddlers' tap cinder returned from Staffordshire. Charges without it, with coal-measure shale for a fluid cinder, made the first "Bessemer Pig" (pp. 178-179, 289).
- At Sheffield: tool steel from Swedish pig; mild steel from hematite pig with Franklinite pig of about 11 % Mn "greatly preferred for deoxydising steel derived from British coke-made iron" (p. 194). Fire-clay tuyeres and "the ganister used for lining the vessel and ladle" were shown in 1861 (p. 203).
- Scrap melted down a coke furnace takes about 2 % C and lacks silicon, "that necessary heat-producing element", so it will not blow hot (p. 293).
Manganese, spiegel and ferromanganese (pp. 256-295)
- Manganese in steel was old: Heath's carburet of manganese of 1839 made weldable cast steel from British iron; no British coke iron was crucible-melted without it (pp. 260-261, 264, 281-282).
- His 1855 patent covered recarburising "by the addition thereto of molten pig-iron" (p. 258), and testing by "dipping out a sample with a small ladle"; "if too much carbon is retained, the pipe G may be again introduced for a short time, or a small quantity of scrap iron may be put into it; but if too much carbon has been driven off, an addition may be made of some melted iron from the finery or cupola furnace" (p. 270).
- Additions in the vessel: fluid metal poured "through an opening in the converting vessel, so that it may fall direct into the fluid mass below"; solid metal heated in the upper chamber and pushed in with a rod; salts and oxides at the tuyeres (p. 268).
- Blowing on to soft iron "had the disadvantage of consuming from 2 to 3 per cent. more iron than when steel was made; and ... the metal got very much overcharged with oxygen, causing violent ebullition in the mould" (p. 268); hence "decarburising only to the extent necessary to make steel of the precise quality desired", as in Sweden and Austria (p. 271).
- Spiegeleisen: "4 per cent. carbon, 8 per cent. manganese ... and 86 per cent. of iron" (p. 271); Hewitt: English spiegel "seldom exceeding nine per cent." Mn with 4-4.5 % C (p. 273). Franklinite pig 11-11.5 % Mn (p. 273). For mild plate he wanted "60 per cent. of manganese, 4 of carbon, and 36 of iron" (p. 271); the first ferromanganese, from a reverberatory gas furnace, ran 20-25 % Mn (p. 288).
- Sweden: pig of 1.9-2.9 % Mn from magnetic ore gives steel "without the use of spiegeleisen, which is not at all red-short"; a fixed vessel with about nineteen horizontal tuyeres "inclined a little from a radial direction so as to give a rotary motion" (p. 275). Metal "run direct from the blast furnace and blown to steel in a fixed converter; no spiegeleisen or re-carburation was needed" (p. 276); an ingot cast "within fifteen minutes of its leaving the blast furnace" (pp. 224, 278). Neuberg ran a pair of three-ton vessels on direct metal of 3.46 % Mn and recarburised with the same pig (p. 276).
- Red-short steel "crumbled away under the hammer if raised to a welding heat" (p. 281).
- A crucible for very low steel stands only one or two meltings (Holley, 1862, quoted p. 337).
Ladles
Pages are printed.
- The casting ladle is "loamed-up", with a bottom discharge valve worked by a hand lever, hung from a hydraulic crane (pp. 148-149); a lip pour curves toward the mould side and carries floating slag over (p. 149). Ganister lines vessel and ladle (p. 203). No capacity or crew is given.