Hamilton, Bolt, Nut and Rivet Forging (1914)
Books Bolt, Nut and Rivet Forging
Covers D. T. Hamilton, "Bolt, Nut and Rivet Forging" (Machinery's Reference Book No. 113, 1914, 52 PDF pages). Pages below are the book's printed folios, which are the PDF page less four. PDF pages 2-4, 6, 48-49 carry no text layer (covers, a blank, the publisher's advertisement). The whole book was read: bolt heading machines (pp. 3-19), continuous-motion bolt and rivet headers (pp. 20-30) and nut forging machines (pp. 31-43), the last bolt-only. The figures of the machines and dies (Figs. 2, 3-5, 6-7, 24, 26, 29, 30) were read from the image, and Tables I and II were read off 300 dpi renders, since their text layer is garbled. Subject heading machines and their dies for bolts, rivets and nuts, and the wear of their tools; bolt and nut practice is marked bolt-only where it does not bear on rivets.
What the book says
Machines and their range (pp. 3-6)
- Headers are stop-motion or continuous-motion. Stop-motion headers "have the greatest range" and head bolts and all upset forgings; continuous-motion headers head "only ... rivets, carriage bolts and short lengths" of machine bolts, much faster (pp. 4-5).
- "The universal practice is to shear the bars cold when working a stop-motion header" (p. 5): the blank is cut to length first, then heated at one end and headed.
- Rivets are made "off the bar": a bar heated for about four feet is pushed into the machine, "the moving die acts as a shear and cuts off the blank", which is gripped, headed and ejected, "in one revolution of the flywheel" (p. 5).
- A plain bolt and rivet machine is two gripping dies, one movable and one stationary, and a ram carrying the heading tool, run by a foot treadle (p. 5). Fig. 2 (p. 5) and Fig. 24 (p. 20) show a cast box bed, a crankshaft across it with a large flywheel or pulley at each end, and the ram working horizontally along the bed; the Ajax header of Fig. 26 (p. 22) is geared, a large spur gear on the crankshaft driven by a pinion.
Heading bolts in a plain header (pp. 6-10; bolt-only)
- In plain dies the bar is turned between blows: a square head takes two or more blows in each of two positions, a hexagon head "at least six blows" (p. 6). The operator keeps his foot on the treadle while the machine repeats, and lifts it to stop with the dies open (p. 9).
- The railway shop of Fig. 9 cuts bars to length in a power shear, heats one end in an oil furnace "as close to the forging machine as possible", and the heater hands each bar to the header operator; "the dies and heading tool are kept cold by means of a constant stream of water" (pp. 9-10).
- Double-deck three-blow dies give a bolt one blow in the lower impression and two in the upper, "free from fins and burrs" (p. 11). The hammer header forms the head with an upsetting punch and four side hammers, three to five blows, and takes longer to change dies (pp. 15-19).
Grip and relief (pp. 11-15, 21)
- A foreign body between the gripping dies would break the machine; a shearing pin in the die slide, or on the National header a spring relief, lets the dies stay open while the ram completes its stroke (pp. 11-13).
- The wedge grip locks the movable die "so that the work can be produced without fins and burrs", and the dies need not be set ahead, which prevents "the pounding or battering and premature wearing out of the dies" (p. 15).
- In a continuous-motion header, if the dies separate "it causes the shank of the bolt or rivet to become tapered or out of round, and also results in fins" (p. 21).
Continuous-motion headers (pp. 20-28)
- Hand-fed: a bar heated for four or five feet is fed through a shear in the faceplate block; the movable die cuts off a blank and grips it; the ram heads it; a kicker ejects it "through a chute, into a box". "The machine runs continuously until the heated portion of the bar has been exhausted" (p. 20).
- Such a rivet "receives only one blow" (p. 20); "it is impossible to produce parts which cannot be completed in one blow" (p. 28).
- The gripping dies carry four interchangeable grooves, "so that when one groove wears out, it is only necessary to turn the blocks" (p. 21); the Ajax dies are turned end for end (p. 22). The gripping dies are made shorter than the blank "thus allowing for sufficient extra stock to form the head" (pp. 21-22).
- Roll feed (pp. 22-25): four grooved rolls draw the bar through a guide pipe and a steel-bushed shearing die; Fig. 29 (p. 24) shows the cycle - bar fed to the stop, the movable die shears the blank and carries it into the stationary die's groove, the heading tool upsets the head, an ejector pin pushes the rivet out. The feed length comes off the crankshaft by connecting rod, ratchet and pawl (p. 23).
- The heating furnace stands 3.5-4 ft from the feed rolls and is "as a rule, 30 feet long, so that the entire length of a bar can be accommodated"; the operator draws the hot bar with tongs, puts it in the rolls, presses the foot lever, and rivets are made "at the rapid rate of forty to seventy pieces per minute" (p. 25).
- Rivet stock: steel of 0.10-0.12 % carbon "is more frequently used than wrought iron, although the latter material is used in considerable quantities" (p. 25). Wrought iron is heated "to almost a white heat", the mild steel "to only about 1400 degrees F., a bright red color"; a head carried far into the tool needs a hotter bar "to make the metal flow more readily and prevent buckling" (p. 27).
- A handwheel moves the stop while the machine runs: an over-size bar gets a shorter feed, and a hotter bar "is upset more on the end by the rolls ... than when the bar is not so hot, and consequently harder"; the operator "watches the pieces as they drop" and keeps "a full head and without flash" (p. 27). The chilled iron feed rolls are water-jacketed, and the dies stay open for much of the revolution to be "well flooded and cooled" (p. 28).
Dies (pp. 11, 29-30)
- Gripping dies are "made from blocks of tire steel", each of three pieces (p. 11); the double-deck die is six blocks bolted and keyed (p. 29).
- Die steel is 0.60-0.80 % carbon, hardened and drawn "so that a file will just take hold"; the heading tool, small and heavily loaded, "must be much tougher" and is 0.40-0.50 % carbon, drawn further (p. 29).
- Bolt dies are drilled with a liner of 1/64 to 1/16 in. between the halves so they grip the bar; rivet dies are drilled to exact size for bar rolled 1/64 in. under, "the expansion of the iron in heating gives sufficient grip", since the work "is practically held in a box" by the dies and the shear (pp. 29-30).
Stock for heads (pp. 19, 28, 30)
- "To produce the head requires considerably more metal than the thickness of the head because of the increase in diameter" (p. 19). Table I (p. 18, bolt-only) gives the bar length for the head: for a 1 in. bolt, 2 3/8 in. for a U. S. standard hexagon head (1 5/8 in. across flats) and 2 3/4 in. for a square one; for a 1/4 in. bolt, 1 3/32 in., over four diameters. "The stop can afterward be adjusted to suit" (p. 19).
- For rivets the excess stock X "is generally obtained by trial", because "no standard for rivet heads is universally followed", and "the scale of the furnace, depending upon whether gas, oil or coal is used for heating, so changes the amount of stock required that a special setting of the stop in different cases is required" (p. 30). Table II (p. 28) gives head proportions but no X column. For a 1 in. rivet it lists a button head 1 3/4 in. across and 3/4 in. high, a steeple head 2 in. by 1 in., a pan head 1 3/4 in. under, 1 in. on top and 7/8 in. high, a countersunk head 1 27/32 in. at 80 degrees and 1/2 in. deep.
- Worked from Table II's proportions (the book gives no X), the head takes 1.43 diameters of bar for the button, 1.33 for the steeple, 1.70 for the pan and 0.54 over the shank for the countersunk; the proportions scale with the diameter, so the ratios hold across the table.
Nut machines (pp. 31-43; bolt-only)
- The hot-pressed nut machine shears, crowns and pierces a nut from rectangular bar, 40-70 a minute, and wastes the wad and the corners (pp. 31-34). The bar is inverted after each stroke so the fin and the rounded corner fall on alternate sides, which saves the end crop (pp. 34-35).
- Fins on the nuts come from "the sharp edges of the cut-off tool becoming rounded"; "when the tools are new the burr or fin produced is very slight, but it increases as the tools wear", and a burring machine removes it (p. 35).
- Nut dies "are usually made from chilled iron castings ... it is claimed, will last fully eight times as long as those made from ordinary carbon steel", though crucible steel of 0.90-1.10 % carbon and vanadium steel are used instead (pp. 39-40); vanadium dies last "about six times the life" of high-carbon ones (p. 40). The four-piece square-nut dies can be raised, lowered and reversed, "giving long life for one redressing" (p. 41). The hot-forged machine's tools "do not wear out nearly so quickly" as the hot-pressed machine's, "owing to the fact that there is not the same scraping action" (p. 42).