Johnson, Principles, Operation and Products of the Blast Furnace (1918)
Books The Principles, Operation and Products of the Blast Furnace
Covers J. E. Johnson Jr., "The Principles, Operation and Products of the Blast Furnace" (1918, 588 PDF pages). Pages below are the book's printed folios: the PDF page less 20 for PDF 21-72, less 32 from PDF 85 on, where plates are inserted. PDF pages 2-4, 6, 12, 73, 76-77, 80-81, 84 and 584-587 carry no text layer (front matter, plates, the last leaves); figures are read from the text that describes them. Read: ch. I (the furnace's parts), III (the two thermal equations, critical temperature, hot blast), VI (slips, voids, the charcoal hearth), VIII (fuels), IX (iron in slag, slag per ton), X-XV (burdening, the burden calculation, distribution, rate of driving, handling, irregularities), and XVII-XIX by search for the grades. Skipped: the chemistry of ch. II, IV-V (solution loss past its conclusions), VII, most of IX's viscosity work, XVI (gas combustion), Commercial Considerations. Stove and stack construction belong to Johnson's Blast-Furnace Construction in America. Subject the operation of the blast furnace - burden, fuel, blast, driving rate, blowing in, the chill and its recovery, slag and pig.
What the book says
The furnace (pp. 2-4)
- Hearth, bosh and shaft; combustion takes place through the bosh, hottest right around the tuyeres (pp. 2-4). The stock is kept up to the stock line (p. 2).
Critical temperature and hot blast (pp. 30-51)
- The critical temperature is the free-running temperature of the slag: 2750 F (about 1510 C) in general (p. 32), 2700 F (1482 C) for a good Bessemer coke slag, 2300 F (about 1260 C) for a charcoal slag (p. 50). Charcoal practice's critical temperature is several hundred degrees lower (p. 41).
- "Lime gives heat to the furnace" is confirmed, and black cinder is often the hotter (p. 40).
- Hot blast cut soft-coal fuel by more than half (p. 31). Clyde Iron Works on cold, 300 F and 600 F blast: 8 t 1 cwt, 5 t 3 cwt, 2 t 5 cwt of fuel, 3.42 : 1.56 : 1, about a 72 % cut (p. 39). A charcoal furnace going from cold to hot blast used fuel as 1.7 : 1 (p. 39); blast heat did little for charcoal, which needed more fuel down in the hearth (p. 47).
- Moisture costs about 20 % more fuel in summer than in winter (pp. 31, 38); 10 % per 0.5 lb of water per 1000 cu ft of blast (p. 368).
- Hearth heat per 100 lb of iron: 1300 BTU for charcoal against 1000 for coke; slag 500 lb per ton of iron on charcoal, 1200 on coke (p. 48). A charcoal furnace fluxes with about 400 lb of limestone per ton at 50 % ore yield (p. 51), about 8 % of ore and stone.
Mechanics (pp. 118-128)
- The blast passes through the coke voids only, about a quarter of the hearth area (p. 118).
- A slip: a local obstruction dams the gas, the pressure under it rises and packs it against the walls, the stock below keeps settling until a cavity forms under the plug; slacking the blast lets it fall (pp. 122-123).
- A cold-blast charcoal furnace is "barely able to avoid freezing up": its combustion temperature is little above the free-running temperature of iron and cinder (p. 128).
Fuel (pp. 170, 183-186)
- Good coke never crushes in the furnace; stock pressure never passes 35-40 lb per sq in (p. 170).
- Charcoal is "almost an ideal furnace fuel": about 69 % fixed carbon, less fuel per ton than coke, porous and fast-burning per sq ft, too weak for large furnaces (p. 183).
- Anthracite was the principal American fuel until about 1860: dense, spalls, needs high pressure, scaffolds (pp. 184-185). Raw dry bituminous coal was used extensively and is still mixed with coke; it fails through low porosity and tar that obstructs the gas and scaffolds (pp. 185-186).
Slag (pp. 200, 219-220)
- Charcoal furnaces run any fusible slag of 40-60 % silica (p. 200), 400-500 lb per ton of iron, about half of coke practice (p. 219).
- Iron in slag: white slag under 0.1 % Fe; 1 % Fe is dark brown or black; a cold furnace 5-7 %; a furnace in a mess about 25 % (pp. 219-220).
Burdening (pp. 243-275)
- Silicon is controlled first by temperature, then by the slag; lime raises the slag's temperature and so the iron's (pp. 243-244).
- Lime to silica 1.3 foundry, 1.4 Bessemer, 1.5 basic (p. 263); limestone is 49 % efficient (p. 264).
- The coke charge is held constant and the ore varied (pp. 265-266). The yield is 102-103.5 % of the Fe charged into pig of at most about 95 % Fe, with about 3 % lost to the flue (p. 265).
- The worked burden on ore A: 9000 lb coke, 19,800 lb ore (2.2 : 1, basic), 4695 lb stone, about 10,160 lb iron; on ore B 6145 lb stone and 5665 lb slag to about 10,100 lb iron, about 1.8 : 1 iron to slag; the foundry burden is 2.0 ore to coke with 2875 lb stone (pp. 268-271). Stone is 14-24 % of ore and stone together.
- About 1 lb of coke per lb of iron (p. 246); 1700 lb per ton in the best practice, 2100-2200 commonly. Each extra 100 lb of slag per ton costs about 35 lb of coke, and 3000-3500 lb of slag per ton is the practical limit (p. 275).
- Without chemistry the slag is judged by its fracture in a small chill mould, the depth of the glassy skin, and lime added or taken off by eye (pp. 260-261). The furnace holds 3-4 h of heat in reserve; a lime change takes about twice as long as an ore change to come through (pp. 261-262).
Distribution (p. 287)
- Ore and coke go in separate layers, thicker being better up to a limit; a coke layer is about 2 ft in a 22 by 90 ft furnace, and a four-barrow charge cost 5-6 % more fuel than a two-barrow one (p. 287).
Rate of driving (pp. 302-313)
- At most about 250 lb of coke per sq ft of hearth per hour (p. 303). Pressure follows the blast volume: 45,000 cu ft per min needs 13 lb, 55,000 needs 17.5 lb (p. 302). The blast crosses the stock in about 2 s (p. 304).
- Radiation and water losses are 15-20 % whatever the rate: at 15 % of the normal rate no iron is made, at 30 % nearly twice the fuel is burnt (p. 306).
- A spontaneous speed-up from solution loss runs the furnace off cold (p. 310).
- A furnace too hot "won't take the wind": pressure rises and it hangs. The remedies are more blast, cooler blast, more burden (pp. 311-312). Slow driving scaffolds (p. 313).
Handling (pp. 314-341)
- Slag is flushed at a cinder notch well above the iron, two to five times a cast; some charcoal furnaces tap the cinder with the iron only (pp. 314-316). The hearth holds the iron between casts, four casts a day (pp. 316-317). Slag rising round the tuyeres raises the blast resistance and slows the driving (pp. 314, 317). Taps are stopped with fireclay (p. 318).
- A furnace runs "literally for years at a time" (p. 323). A furnace let down loses its top-gas heat and its later charges arrive raw (pp. 324-325).
- Blowing in: cold stock and cold walls, so a coke blank of a quarter to a third of the height goes in first, then light burden on a coke charge two to three times normal, the burden rising toward the top to 1 : 1 ore to coke, half the normal burden (p. 326). First cast after 24-48 h, normal burden after one to two weeks, blast about a third of normal (pp. 326-327). Lighting at the top was "absurd"; the furnace is lit at the tuyeres with oily waste (pp. 328-329). A slow fire drawing up the shaft leaves material half-molten and sticky, so a quick blow-in is better; double blast for a few minutes starts the stock settling (p. 329). Old slag goes in at blow-in (p. 332).
- The tap hole is left open with a 4 in pipe so the gas blows down and "burns fiercely out the end of this pipe", warming the bottom and the iron trough; it is stopped when cinder comes (p. 331).
- Banking: the losses go on while no iron is made, iron left in the hearth freezes, and air drawn in at the tuyeres burns the coke unless they are sealed; before a stop, cast everything and charge a coke blank to the tuyeres (pp. 333-335). Iron frozen round the tuyeres after a stop is low in carbon, "almost like wrought iron" (p. 334).
- Blowing out: the top gas grows hotter as the stock falls; the old practice left a flame 100 ft high. The burden is lightened so the last iron taps hot; iron below the tap becomes the salamander (pp. 336-337), 250-300 t at about 1.5 % C that "could almost be forged" (pp. 338-341).
Irregularities (pp. 346-368)
- Regularity above all; a filling stop of one or two hours sends raw charge down (pp. 346-347). Among the causes of derangement: "charging ore without sufficient fuel" (p. 348).
- Slips are met first by slacking the blast (pp. 348-349); explosions follow when the fuel bed burns out under a suspended column (pp. 349-352). Scaffolds are cleared with a light burden, silica on coke furnaces and lime on charcoal ones (pp. 350-353).
- The chill: raw material in the hearth turns the cinder "black as tar"; the tap hole is lost and the furnace is cast through the cinder notch (pp. 353-356). The cure is a coke blank charged at the top, 8-20 h working down, with the burden lightened; "the wise furnaceman when he sees signs of impending trouble, charges a good blank" (p. 355).
- A chilled hearth is opened with dynamite, a kerosene burner, an electric arc or an oxygen burner (pp. 357-363). Solid lumps of coke, ore and stone are pulled out through the tuyeres and the cinder notch, fresh coke packed in from outside, lit and blown (p. 363). "A furnace is never in vitally serious trouble until it becomes impossible to remove the molten materials from the hearth" (p. 364).
Products (pp. 440-444)
- Gray forge for puddling: 0.75-1.25 % Si, 0.3-0.4 % P (pp. 440-441). Graded by fracture No. 1 to No. 6: No. 4 gray forge, No. 5 mottled, No. 6 white (p. 444).
Ladles
Pages are printed.
- Hand ladles take slag samples; slag poured from one falls in pellets or strings (pp. 144, 202); iron settles in a slag ladle on its journey to the dump (p. 219).
- Slag is carried molten "in ladle cars", and "end dump ladles" build fills (pp. 516-517); ladle-handling cranes transfer hot metal (p. 439). No cinder box, bogie or slag pot is named.