The founder's air furnace (Biringuccio, 1540) and the Stueckofen

Books Metallurgy: Iron and Steel, The Manufacture of Iron

Covers period texts read as archive.org OCR text. Page numbers are printed folios read from OCR running heads; OCR is rough, so every figure from a bad scan is marked OCR.

  • Air furnace:
    • V. Biringuccio, De la pirotechnia (Venice, 1540), Italian original, archive.org delapirotechnial00biri (the 1550 and 1558 editions pirotechnialidie00vann agree where compared). The Smith and Gnudi English translation (1942) was NOT read: every Biringuccio line below is the note's own reading of the Italian, with the leaf ("car.") numbers of the 1540 table of contents. Book VI (moulds, bells, cannon) and Book VII ch. 1-7 (furnaces, melting).
    • Lord Grimthorpe (E. B. Denison), A Rudimentary Treatise on Clocks, Watches and Bells (London, the 1874 printing, archive.org arudimentarytre01grimgoog), pp. 351-353, bell moulding and melting; 19th century practice.
    • A. Ure, Dictionary of Arts, Manufactures, and Mines, vol. 1 (7th ed., 1875, dictionaryofarts01ureauoft), arts. Bell-metal (about p. 335) and Bronze (pp. 536-538).
    • J. Percy, Metallurgy: Fuel ... Copper ... (1861, metallurgyartofe00percrich), Welsh copper melting furnace pp. 318-322.
  • Stueckofen:
    • J. Percy, Metallurgy: Iron and Steel (1864), read from the archive.org OCR metallurgyartex02percgoog. pp. 319-320 (introduction) and 326-329 (the Stuckofen).
    • L. Beck, Die Geschichte des Eisens, Bd. I (1884), archive.org diegeschichtede05beckgoog, pp. 816-825 (Die Stueckoefen); Bd. II, diegeschichtede03beckgoog, pp. 170-173 (OCR of this volume is bad).
    • F. Overman, The Manufacture of Iron (the 1854 printing, 10293241bsb; the first edition is 1850), pp. 141-142, "Stuck, or Wulf's Oven".
    • Not reached: Jars, Voyages metallurgiques (1774, the primary Eisenerz account; Percy and Beck quote it), Swedenborg De ferro (1734, via Beck and Percy only), Johannsen, Swank, Diderot's Encyclopedie articles and plates on cannon and bell founding.

Facts are the sources'; INFERRED marks the note's own reading.

Units, all INFERRED (no source read gives them): Tuscan braccio about 0.58 m; Styrian/Rhenish foot about 0.31 m, 12 in to the foot; Wiener Zentner (Ztr) about 56 kg; Percy equates the German quintal/centner to the English cwt (50.8 kg) "in this case"; Elle about 0.6-0.8 m (not fixed).

A. The founder's air furnace (reverberatory), Biringuccio 1540

Biringuccio writes "fornace a reverbero" and "fornace potentissima" (VII, ch. 1, car. 101-103). Bronze, cannon and bells are melted in it with wood flame; his other four ways (basin, "cestone", ladle, crucible, wind furnace, ch. 2-4, car. 104-106) use charcoal and bellows and are for small lots or for alloying copper first.

A1. Why a reverberatory furnace

  • "Fornace potentissima che si chiama di reverbero", chosen "not only for convenience" (car. 102). Needed when the melt is large; a single furnace may still not be enough: Leonardo planned the Sforza horse "with the fusion of three furnaces at one time", and a Flemish master needed two furnaces for one bell because one failed (car. 102).
  • Founding is "tutto il fine dell'intento vostro": he names four needs: the furnace, dry wood or charcoal, a charge disposed to fuse, and the founder's judgement (Prohemio, car. 101).
  • Fine copper alone cannot be melted in it: "se pensaste di fondere in forno di reverbero rame fino da per se ... vi crepareste l'anima"; copper "vuol fuochi repentini e gagliardi, con vento grande e violento" so it is first melted with bellows and charcoal (basin, ladle, or crucible) and brought to the reverb furnace as an alloy (VII ch. 6, car. 109). INFERRED: so the reverberatory furnace takes bronze or pre-alloyed copper, not raw copper.

A2. Plan, as he laid it out (VII ch. 1, car. 101-103)

  • He rejects the makers' many shapes: round like a bread oven, oval across the fire entry, oval along it; one, two or three flue-windows; fire entry high and narrow or wide and low; fuel put in by the flank, along the length, or from a hole above. "Tanto varie ... quante quasi sono il numero de maestri" (car. 101). Round pleads that every line runs to one centre like a burning-mirror; long pleads more united flame over the metal and an easier hearth to work (car. 103).
  • His own plan is drawn on the ground first. For a hearth "di un diametro di due braccia e mezzo" (2.5 braccia, about 1.45 m, INFERRED) he draws a line "lunga braccia tre e mezzo, o tre e due terzi" (about 2.0-2.1 m), a cross-line of 2 braccia at the end of the arms ("due braccia"), and the fire-entry line two-thirds of a braccio long. The hearth comes out "quasi a forma d'un leuto" (like a lute) (car. 102). OCR is broken here; the cross is the window arms.
  • The flame windows ("finestre", the exhalers) sit at the ends of the cross arms. In the wall they are flared "a guisa di bombardiera" - wide outside, narrow inside - and are arched (car. 103).
  • Foundation: walls drawn "grosse" a braccio or three-quarters of a braccio at least from the floor up; the solid wall is raised from the fire-place outward "alto sopra a terra fino un braccio"; hollow parts are filled with rubble and earth rammed with pestles to save cost (car. 102).
  • Floor: bricks laid over a platform, falling toward the tap by "un quarto di braccio o meno" so the bronze cannot rest but all runs forward; over that a second course of bricks set on edge ("a spino per taglio") with sharp-cornered bricks chosen and rubbed to fit tight (car. 102).
  • Tap: two bricks are cut so a pyramidal iron pin ("spina del ferro piramidata") seats in them, thicker toward the bronze so the load of metal pushes it shut (car. 102).
  • Fire-box: "una gran fossa cupa e lunga quanto tutto il forno", half a braccio lower than the floor of the fire entry; across it "architetti attraversati" (cross-bars, the grate) three fingers apart and sloping, one-third to one braccio fall toward the stoking mouth ("bocchetta dove si mettono le legna") (car. 102). OCR; the grate slope figure is uncertain.
  • Inside, the walls narrow toward the fire entry and widen toward the metal so the flame is forced forward and enters "all united" at the bronze place; the stoking vault is lower than the melting vault; the vault over the metal is low, "da el piano di sotto alla maggior sua altezza un braccio e un quarto" (about 0.7 m, car. 102), to keep the flame and heat close to the bronze; the rooflines slope with the floor so the flame does not stand in the high part and turn back to warm the floor instead (car. 102).
  • Bridge/baffle: a low arch between fire and metal; from the arch floor to the fire-entry floor half a braccio; the wall between wood fire and bronze is three-quarters (of a braccio) over the arch (car. 102). OCR, read with doubt.
  • Flues: the two windows give two small chimneys ("caminetti") in the thickness of the wall, each opened about an eighth ("ottavo") to take smoke out; each window has a clay shutter in an iron frame that can be lifted off and set on (car. 102-103, 107).
  • Walls and lining: fired brick, or if raw brick then stone that stands fire; in the part the fire reaches, bricks laid in white fire-clay as glassmakers use for their pots and furnaces; peperino stone and a black blistered tale-flecked stone from Brescia, Chiusdino (Siena), Bolzena, the Tolfa alum works are named (car. 103).
  • Two fire mouths: if one flame trumpet is too small a mouth for a great hearth he would make two stoking mouths, each throwing flame to the metal and meeting before it ("si congiungessero e divenissero una") - if they met head on they would offend and block each other's flow (car. 102-103; a drawing of the hearth bottom follows).

A3. Preparing and heating the furnace (car. 103, 107)

  • A new furnace is fired thoroughly with charcoal and wood before any bronze goes in, the floor most of all, "che si non e ricotto facilmente potrebbe che non fondesse".
  • A cracked floor is mended with lime and brick dust or with ground glass, then the whole floor given a wash of lye-ash slurry "che difenda dalle fiamme"; stone is kept from burning, brick from running.
  • Tap hole stopped with the ash-coated iron pin; charge set "larga e piu per ritto delle fiamme che potete".
  • The charge lies on bits of brick so the floor is "sospesa" by an eighth, letting flame get under and heat the floor before the bronze melts.
  • Both windows stopped with their clay shutters, leaving peep-holes; "E col nome di Dio" the fire is begun with wood on the mouth of the fire entry, and drawn forward "a poco a poco" to the line of the flame windows; then fed with more and more wood vigorously, the fire never slackened until the charge goes red, white, and begins to fuse.
  • Fuel: "legno giovane secco", flame-giving rather than coal-making, and plentiful: "hauer ne debbi fi superfluo", in split pieces not too thick; hornbeam, willow, alder, walnut, beech, and the light porous woods called "dolci". A damp fuel gives no heat.

A4. The charge and the melt (VII ch. 5-6, car. 107-110)

  • Alloy: he calls "bronzo" anything of copper with tin, brass, or lead; "metallo" the finer: tin "dodici per cento fino a venticinque" - a rich tin bronze, used for bells, mortars, and "lavegi" (car. 110). Bells: "buono stagno, e non habbi in se per alcun modo piombo" - lead spoils the sound and the casting (car. 97). Some masters add a little lead for economy (car. 109).
  • Order: pigs of one alloy ("pani d'una natura") melt together and quickest; if the lots are mixed (copper bits, old kettles, pots) he puts the good alloyed metal in first, then adds the scrap little by little, each piece warmed at the mouth before it goes in so as not to chill the bath (car. 108-109). Tin goes in last, "quella quantita di stagno che penserete che meglio il corrompa" (car. 107).
  • Working the bath: through the tap-side peep or the door, a chestnut pole ("castagnolo") rakes the floor, breaks the crust ("pelle") that strong dry flame throws on the metal and that stops heat reaching below it, and also breaks the big pieces so they melt (car. 107).
  • Test of readiness: a sample is drawn with a hollow cane or a small ladle ("cazzetta") to judge; it must be "liquida come acqua o olio", the bath flat, scum floating, "lampeggi come il sole", and the flames from the vents almost white and smokeless (car. 107). More tin is added if the sample asks for it. A fat of pig or other animal with tartar or saltpetre is thrown on, or sheep's horns, to clean the bath, with another heat (car. 107).
  • Skim: "coll'ariscio di legname o di ferro" take out slag, earth, and brick pieces used for suspending; skim the dross (car. 107).
  • Danger of slow melt: "se lo date un mese di fuoco non lo fondereste" (car. 108); scrap fused after a lump of good alloy cannot be rescued by waiting. No melt time in hours is given in the book. INFERRED: a long, careful heat; the text gives no quantity per heat, only that a great mass may need two or three furnaces at once.
  • Fuel for hot or large heats is a matter of the master's choice; the helpers' effort is mentioned (car. 107).

A5. Tapping and the channel to the pit (VI ch. 10, car. 90-91; VII ch. 5, car. 107-108)

  • Tap: the founder drives out the plug with a bent iron rod with a long handle ("el mandriano"), pushing the pin of the "spina" inward while holding it in his hand, "temperando con la ponta d'esso messa nel buso" - he regulates the flow by how far he lets the pin out, according to the mould and his judgement (car. 107-108). Cannon are filled with moderation: a rushed fill can break the core or the mould; for guns and bells he lets it run "temperatamente e non repentina" and enough to overflow (car. 97).
  • Channel: "un canale di mattonio docci murato di terra largo un quarto di braccio, alto altrettanto" (about 0.15 m square), bricks or tiles/gutters laid in clay, ash-washed, then fired with charcoal or wood so that when the bronze runs it "non habbia da sentire alla humidezza ne frigidita"; the cup ("coppa") at its end likewise warmed; all cleaned with an iron rod in the tap before running; the metal "come un olio" (car. 91).
  • Channel and pit are laid from the furnace spout: "fra la forma e l'uscita del bronzo del fornello"; when several moulds stand in the pit, the sprues are set against the furnace's outlet and each takes the metal by its own channel (car. 91).
  • Head: when the mould is nearly full he puts more tin into the furnace or over the channels so the "matarozza" (the feeding head / sinking head) is fully fed (car. 108).

A6. The pit and the moulds, cannon and bells (VI ch. 5-14, car. 83-99)

  • Cannon: "essendo forma d'artiglieria ... si deve gittar ritto" (cast upright): a pit ("fossa, ovvero pozzo") dug in front of the furnace, "cupa quanto e la lunghezza della forma, e tanto piu" and with a fall from the furnace spout so the bronze runs easily to the mould; hard at the bottom so the weight cannot sink the mould; the mould set in plumb on a cross/iron-plate ("rotella") and the earth rammed round it "a suolo a suolo di tre dita in tre dita" with pestles, as dry-damp earth ("humida ma non molle"), up to the level of the furnace floor, "tanto che divenga un masso di pietra" (car. 91).
  • The mould is a loam mould of several pieces bound with iron wire and bars, with a separate breech piece, wired and clipped; the core ("anima") is hung with an iron bar in the centre with a spindle, and tied to the frame so the metal cannot lift it; vents and gates stuffed with tow and cloth (car. 86-91). Dried and baked ("ricocer") in the pit; a fire burned round it (VI, ch. 10, car. 89-90).
  • Bells: the loam mould is built up either standing in the pit on a "centino" (a sweep) with the fire inside a hollow pyramid of bricks whose floor has a pit "cupa due braccia tonda" two braccia deep, dried by the fire within; or lying; he prefers lying but both are described (car. 94-97). The core and the "tonaca" (the false bell, which is later broken) are baked in a small brick kiln ("fornaciotto") four fingers off the core and as high as the core, filled with charcoal with flame between core and false bell; then ash-washed and set in the pit before the furnace on a star or cross of timber and iron or wood hoops so the core cannot move; the pit "cupa tanto che tutta la forma cuopra" and hard-bottomed, the bottom of masonry or of walnut/alder wood planks; the pit filled with earth beaten in with mallets a little at a time (car. 96).
  • Pour: "fondendo e facendo un canale, aprendo con il mandriale il forno, quando il metallo e fuso empirete la forma" (car. 96). Small bells need fewer bindings; big ones need hoops, irons and cords and a "temperata" pour without a rush, enough to overflow (car. 97).
  • Cooling: some masters take the bell out hot and it cracks; others bury it "tanti giorni ... quante migliaia di peso contengano" - roughly one day per thousand pounds (OCR, car. 98). Bells improve over the first year from hammering of the clapper (car. 98).
  • Scale: one bell cast in a "cestone" (basin-pit furnace) at Palermo weighed "circa 10006" pounds - OCR, probably 10,000 (car. 105). Savoyard and French itinerant founders use the same "catino/cestone" with two or three pairs of bellows round it and with a brick tower in place of wattle (car. 105).

A7. Blast, if bellows are used (VII ch. 7, car. 111)

  • Bellows for the basin and crucible ways: soft, with ample cloth, long and wide leather, good long nozzles, tight; he gives hand and water drives. Water: a water wheel ("ruota a bottacci", fed from a pond) "di diametro 6, 7 et 8 braccia" with two cross cams set in opposition, pressing the bellows boards, the top board fixed, the lower raised/dropped by the cam (car. 111, OCR partly lost). So the same shop could run a water-blown pair of bellows for the charcoal furnace beside the wood-fired reverb furnace. INFERRED: the reverb furnace itself takes no bellows; draught is the chimney and the windows.

A8. Faults and cautions

  • Furnace floor cracks if not baked; a melt is "pasty" and the crust sealed if the fire is dead; a stuck piece of copper in the hearth can freeze a whole charge; the mould floor must not give; the core must not float or move; too-hot metal gives a "crude and harsh" tone (car. 97); lead in a bell; tin lost to oxidising when held long at heat (Ure, below).
  • Founders disagree: "ognuno ... secondo li suoi pareri" (car. 101).

A9. Later practice, as compared (19th century)

  • Ure, Bronze (p. 537): "The bronze founder ought to melt his metals rapidly, in order to prevent the loss of tin, zinc, and lead by their oxidisement. Reverberatory furnaces have been long used for this operation, the best being of an elliptical form. The furnaces with dome tops are employed by the bell founders, because, their alloy being more fusible, they do not require so intense a heat." Charcoal or coke on the melting surface; tin put in last and "thrust to the bottom of the melted copper"; stir, then pour at once; cool the casting fast to avoid separation.
  • Ure alloys: bell-metal copper 78 tin 22 (Bronze, p. 537); the older bell-founders aimed at 3 copper to 1 tin (Bell-metal, p. 335); 3.5:1 favoured; 4:1 for house bells; cannon metal about 90-91 copper to 9-10 tin (12 to 14 of tin to 100 of copper from Turin, 1770; 8 to 11 from Douai, 1786) (p. 537).
  • Denison (Grimthorpe), pp. 352-353: "Bell-metal ... is melted in a reverberatory furnace, in which the fire is at one end of a long shallow trough which holds the metal, and the flame is drawn over it to reach the chimney at the other end, and is reverberated down upon it from a 'bridge' or a low roof over the trough." Whitechapel "still use wood"; old founders probably wood, "unless they used charcoal, as I understand they do in Russia"; wood takes long to bring up the heat and "it is notoriously a bad thing to keep the metal long melted getting up the heat"; Woolwich gave up wood for coal or coke for gun-metal; bells always cast mouth downward; the cope weighted with earth in the pit; one hole for metal, another for air (p. 351-352). A 12 cwt bell: the coal-cast one beat the wood-cast one; Mears's Westminster bell took "nine times as long in the furnace" and four times as long running (p. 353).
  • Percy 1861 Welsh copper melting furnace (pp. 318-322), a reverberatory furnace with dimensions only in its figures (not in text): large fire-place with ash-pit; fire-bridge with a narrow gap and a cast-iron bridge plate; arched chamber below carrying the bed; sand bed "about a foot ... total about 20 inches" (12 in in some works), shaped into a shallow cavity falling to the tap hole, sintered by melting slag on each layer; fireplace "very large compared with that of a calciner"; coal fed through an open mouth kept closed with coal; inner walls, roof and stack of fire-brick, outer of common brick, Dinas brick in the roof; a hole in the roof with iron hopper to charge; an end door by the stack for rabbling and slag with a peep-hole; the stack braced with iron rods (p. 318-321).

B. The Stueckofen (Styrian-Carinthian high bloomery)

Names: "Stuck- or Wolfsofen" because the lump (Stueck, Wolf) is drawn out at the bottom (Percy p. 320). "Blauofen" also used - "plaa" = to blow, workers "Plaaer" - and later applied to the blast furnaces that replaced it (Beck I p. 816-817; Percy p. 329). Percy: "for which there is no English name, but which might be called the high bloomery furnace, as it is only a Catalan furnace extended upwards in the form of a quadrangular or circular shaft" (p. 319-320).

B1. Dates and places

  • Beck I p. 817-818: "Angeblich sollen sie schon im 8. Jahrhundert in Steiermark bestanden ... Sicher verbuergt ist, dass sie im 13. Jahrhundert in Steiermark in Anwendung waren." In old times they were lower and were raised "nachdem man angefangen hatte, die Geblaese durch Wasserraeder zu betreiben" (p. 817). Eisenerz mine said opened 712 (inscription) (p. 817-818); Leoben iron first in a document 1164 (p. 818).
  • Styrian steel made "seit dem Mittelalter ausschliesslich in Stuckoefen" (Beck I p. 818); first Hochofen at Eisenerz 1750; the Eisenerz Stuckoefen were shut in 1762 against the workers' opposition; at Eisern in Krain until after 1847; at Schmalkalden after 1841 for finery slags; at Windisch in Kaernten likewise; Hungary and Transylvania "bis auf die Gegenwart" (Beck I p. 818).
  • Percy p. 326: formerly in Carniola, Carinthia and Styria; "Karsten, in 1841, stated that on account of their great consumption of fuel they had been entirely abandoned, though they were still in operation in Hungary, and to a limited extent also in Germany, in the district of Henneberg." Beck says at Henneberg it lasted longer than in Styria (p. 817).
  • Overman p. 141: "A few are still in operation in Hungary and Spain. At one time they were very common in Europe."
  • Around 1714 Swedenborg counted 16 Stuckoefen at Vordernberg working spathic ore from the Erzberg (Beck I p. 819). Output 1745 Vordernberg 127,087 Ztr of Halbmasseln plus pig; 5.05 Fass charcoal, 36.5 cubic feet, per Ztr (Beck I p. 823).

B2. Form and inside dimensions

  • Percy p. 327 (Schmalkalden, Quantz 1791): inside "two truncated cones with their broad ends or bases in contact"; height 16 ft (two others 12 ft); diameter at bottom 2.5 ft, at the mouth 1.5 ft, at the widest part "exactly in the middle, or 8 ft above the bottom, 4 ft 2 in"; carried up a few feet above the mouth, "gradually widening for the sake of greater convenience in charging". Beck I p. 824: the 12 ft ovens 2.5 ft wide at the bottom, belly 3 ft wide at 6 ft above the bottom, throat 1 ft 8 in; the 16 ft belly 4 ft 2 in.
  • Karsten (Percy p. 327): height 10 to 16 ft; either regularly wider from top to bottom or, in most, bellied in the middle; round or quadrangular. Beck I p. 820: normal height in Styria in the 18th century 10-16 ft; the lower part mostly rectangular, seldom round, "betraechtlich weiter" than the later Flossoefen; length 4 ft, width tuyere-side to far wall 2.5 ft; older ones under 10 ft; Schmalkalden later 19-24 ft (Beck's figure; Percy says 16).
  • Swedenborg, Vordernberg about 1714: furnace 14 ft high, 4 ft [wide] above the tuyere and 2 ft wide at the throat (Beck I p. 819, wording ambiguous). Larger ones elsewhere in Styria 18 ft, rectangular below, tuyere height 1.5 Ellen, belly 3 Ellen above the tuyere and 3 Ellen across, round above it and narrowing to 1 Elle at the top (Beck I p. 819-820).
  • Swedenborg via Beck II p. 171 (OCR bad): three kinds, large 18 ft, middle 14 ft, small (taken as 10-12 ft, the oldest and commonest); the small ones square below with 2 ft sides, widening above the tuyere to 4 ft about half way up, going round, then narrowing to 1 ft at the throat; he compared the inside to an Italian pitcher.
  • Overman p. 141: "inside has the form of a double crucible ... generally from ten to sixteen feet high; twenty-four inches wide at the bottom and top; and measures, at its widest part, about five feet."
  • Hearth at Eisenerz: "4 ft. wide and 2.5 ft. deep, opposite the twyer" (Percy p. 329); the hearth stone sloped 2-3 in toward the drawing hole (Percy p. 327; Beck I p. 820); rammed from charcoal "Gestuebbe" (Beck I p. 820).
  • INFERRED reading: a quadrangular stack about 4 ft by 2.5 ft at the foot, bellying to 4 to 5 ft, closing to about 1.5 ft at the throat, 10 to 16 ft tall (3 to 5 m), is the whole range the sources give.

B3. Walls, hearth and breast

  • Walls: "aus einem graulichen Sandstein ... an der Basis 4 bis 6 Ellen Seitenlaenge" (Beck I p. 820); inner walls rammed of refractory material and said by Swedenborg to last 12 years (Beck II p. 171, OCR); Schmalkalden flue masonry of sandstone held by six anchors, with a funnel-shaped top for charging (Beck I p. 824). The hearth stone at Schmalkalden was "a siliceous conglomerate" (Percy p. 327).
  • The hearth stone corroded: the tuyere at Schmalkalden stood 14 in above the bottom but after long working the bottom was eaten away until it stood 20 in; "this variation ... had an extraordinary influence upon the yield, the quality of the product, and the consumption of charcoal" (Percy p. 327).
  • The drawing hole / breast ("Brust"): the "characteristic ... of the old Styrian ovens that there was only one opening in the lower part", the same hole through which the lump was drawn also took the blast (Beck I p. 820); it took the whole width, 4 ft wide, 2.5 ft high, mostly in an iron frame; closed with fire-clay bricks ("feuerfeste Thonsteine") (Beck I p. 820-821). Percy p. 327: 2 ft wide, "before the smelting began was stopped up with bricks and clay". Overman p. 141: "The breast is open; but, during the smelting operation, it is shut by bricks; this opening is generally two feet square. The furnace must be heated before the breast is closed."
  • The breast wall was "only one brick thick" (8 in) (Beck I p. 822). A separate slag tap sits left of the tuyere, or at the bellows side about 1.5 ft from the tuyere opening (Beck I p. 821; Beck II p. 172, left of the tuyere hole); in many places the slag ran off continually over a dam ("Damm") on the left of the breast (Overman 1854 p. 147 for the blast furnace; Overman p. 141 for the Stueckofen: "a portion is suffered to escape through a hole in the dam b").

B4. Blast: tuyere, bellows, drive

  • Percy p. 327: one tuyere, copper, horizontal, projecting 3 in into the furnace; "usually made of clay, and rarely of copper" generally (Karsten), "nothing definite as to its width"; at Eisenerz the blast came in on the drawing-hole side, so the bellows had to be removed each time before drawing a lump; "The blast was produced by bellows moved by a water-wheel."
  • DISAGREES: Beck I p. 824 says the Schmalkalden copper tuyere "ragte 3 Fuss in den Ofen hinein" (3 ft); Percy says 3 in. Percy's is the likelier (Beck gives nozzles set back 3-4 in in the tuyere, front diameter 1.5 in, p. 824).
  • Eisenerz tuyere (Jars, via Percy p. 327-328 and Beck I p. 823): a clay brick; Percy "about 4 in. thick ... projecting about 10 in."
    • Beck "10 Zoll Laenge und 4 Zoll Dicke", the other bricks "nur 8 Zoll stark", so it projects 2 in (Beck's figure is self-consistent; Percy's 10 in is likely a slip). A hole is bored with a pointed iron rod through the length: Percy "about 3 in. wide on the outside and 1.5 in. on the inside of the furnace, and about 12 in. above the bottom"; Beck "vorn 1.5 Zoll, hinten 3 Zoll". Clay flanking lumps 8-10 in broad and 2 in thick, joints stopped with clay (Percy p. 328). The tuyere and slag hole were raised as the iron built up (Percy p. 328; Overman p. 141: "tuyeres are generally kept low, upon the surface of the melted iron, which thus becomes whitened. As the iron rises, the tuyeres are raised").
  • Overman p. 141: "There are generally two tuyeres ... at least two bellows and nozzles, both on the same side." Sources disagree with Percy/Beck (one tuyere); Percy 1864 and Beck 1884 draw on Jars/Quantz, so one tuyere is read for the Styrian type. Overman is general and older.
  • Bellows are hung up and slid into place on the tuyere side, driven through lifting cams from the wheel shaft, and must not be so large or heavy that they cannot be taken away before the lump is drawn (Beck I p. 822; Beck II p. 172 on the shaft, "Hebedaumen", OCR garbled); the ore baskets are raised to the top by a simple hoist also driven from the wheel (Beck II p. 172, OCR garbled).
  • Bellows for the lump: the lump is drawn by a chain round a vertical post or cylinder joined to the wheel shaft (Percy p. 328; Beck I p. 822). INFERRED: the water-wheel drives the bellows, the lump hoist, and at some works the tilt hammer.

B5. Preparing, lighting and bringing it up

  • Ore: spathic iron ore of the Erzberg, left in heaps in the air for some years "damit er reif werde", so that sulphur salts wash out (Beck I p. 819, 821); then roasted in heaps ("Gramatteln") of three ore layers over wood and charcoal, covered and burnt, three weeks (Beck I p. 821). Each smelter has a roasting oven beside (Beck I p. 819).
  • Lighting (Percy p. 328): "the drawing-hole having been closed ... the furnace was filled with charcoal, which was ignited through the twyer. The bellows were worked a few times and then stopped, so that the charcoal might be slowly kindled and the furnace heated by degrees. As soon as the fire had reached the top, the blast was again let on, and the charging with charcoal and iron ore commenced." Beck I p. 821 the same: fire through the tuyere, bellows hung on and blown slowly; blast stopped until the glow, by natural draught through the tuyere, has gone through the whole column of charcoal.
  • Overman p. 141: the furnace is heated before the breast is closed, then charcoal and ore thrown in.

B6. The charge, order and proportions

  • Percy p. 328: "At first only little ore was added; but the proportion was gradually increased until the proper relation between the charcoal and ore was attained, that is, about 4 measures of the former to 1 of the latter." Beck I p. 821: the ore charged by measure; the charcoal charge constant, ore charge growing; in low furnaces the ore often pre-mixed with charcoal; "Anfangs gab man nur wenig Erz"; layers.
  • Eisenerz: charged on until 13 tubs of 3.5 Ztr of ore - "das festgesetzte Quantum fuer eine Luppe" (Beck I p. 822, tub figure from OCR, agrees with 320 Ztr per week for 7 lumps, p. 823). The ore charge was carried high so that part of the protoxide of iron from incompletely reduced ore passes into the slag and works as a decarburiser on the iron mass (Beck I p. 822).
  • Swedenborg small Eisenerz ovens: 20 to 24 charges, each 2 Fass of ore and one Mass of charcoal (three making a sack) (Beck II p. 172, OCR).
  • Schmalkalden in the early 19th century charged finery slags and forge and hammer scale with at most a quarter red haematite; the first charges about twice as heavy as at the neighbouring blast furnace, then alternating light and heavy ore charges, the slags let run continually so they never stand over the iron, the tuyere wet and dark all through (Beck I p. 824-825). Karsten's slag analyses: charged slag FeO 84.3 %, tapped slag FeO 51.1 % (Beck I p. 825).
  • No flux is named in Percy, Beck or Overman for the Stueckofen proper (the spathic ore is self-fluxing; Beck I p. 821 says the roasting leaches sulphur, nothing of lime). INFERRED: no added flux is recorded for the Stueckofen.

B7. Slag handling in the run

  • Slag was tapped "through an aperture made in the 'stopping' of the drawing-hole, and this was kept constantly open"; first slag with little iron was stamped and washed to catch cast iron shots; later "when the mass of iron in the hearth became considerable, it was kept hot by allowing the slag to accumulate in front of the drawing-hole; for, otherwise, it was much more difficult to detach, and great damage might be done to the furnace" (Percy p. 328).
  • Beck I p. 821-822: slag first tapped within minutes of the ore reaching the tuyere, at the bellows side; the tap stopped with loam after each run; the tap rose with the iron in the hearth.
  • Probing: the smelter checks through the tuyere whether enough iron has gathered (Percy p. 328; Beck I p. 822).

B8. Campaign length and rhythm

  • Eisenerz: "Die ganze Zeit einer Schmelzung dauerte 18 Stunden, naemlich 15 Stunden zur Schmelzung und 3 Stunden zum Ausbrechen und Teilen der Luppe und zur Vorbereitung des Ofens" (Beck I p. 823; Percy p. 329 identical: 18 hours, 15 + 3).
  • The workers were bound to make seven lumps a week, about 320 Ztr of ore; the ovens "gingen gewoehnlich von Montag frueh bis Samstag Abend" (Beck I p. 823). INFERRED: about a lump a day on a rest of 6 days with Sunday off.
  • Schmalkalden: three lumps a day on average, 60 to 70 centners a week, no work on Sunday, 3 men at a time in shifts of 8 hours (Percy p. 329).
  • Swedenborg, small Styrian ovens: a lump every 6 hours, so 8-10 Zentner in 24 hours (Beck II p. 172, OCR).
  • Overman p. 141-142: "In about twenty-four hours, one ton of iron is deposited at the bottom of the furnace"; blast stopped after a few dead (coal-only) charges. Older, general, and larger than the other sources.
  • INFERRED: not a continuous furnace; the shaft is lit, run to a lump, let down, emptied and repaired each time (see B10).

B9. Drawing the lump and opening the breast

  • Percy p. 328: when enough iron had gathered, "the charging was discontinued and the furnace allowed to go down, or a few charges only of charcoal were supplied, and the slag in front of the drawing-hole was quenched with water and carried away, after which the hole was opened, and the mass of iron after having been loosened from the sides and bottom of the furnace extracted."
  • Beck I p. 822: bellows removed first; an iron plate set at the bottom of the thin breast wall and kept continually wetted to cool it; the clay bricks above the tuyere level knocked out and the unburnt charcoal raked out through the opening, quenched, and reused in the ore roasting; more of the brick wall broken out, slag runs and with it a share of liquid pig iron ("Roheisen") that is quenched with water - 6 to 7 Ztr in Jars's time ("graglach"/"Wascheisen", kept and refined, Beck I p. 823).
  • The lump is bared on all sides, left covered with charcoal in the middle where the steely parts are, to avoid decarburising; crowbars lift it; a large toothed tongs with a ratchet ring and a chain, the chain wound round a post at the far end of the shed and fixed to the wheel shaft, so "dass das Wasser das Ausziehen der Luppe besorgt" (Beck I p. 822). Percy p. 328: "grasped by large pincers and pulled out by means of a chain passing round a vertical cylinder in connection with a water-wheel." Overman p. 141: lifted loose by crowbars, "taken by a pair of strong tongs, which are fastened on chains, suspended on a swing crane", and moved to an anvil.
  • If the mass has partly fused and stuck to the bottom: let the furnace cool a little and detach it "as best could be done" (Percy p. 328); "great damage might be done to the furnace, which, indeed, sometimes happened in any case" (Percy p. 328).
  • Working the lump: covered at once with charcoal dust (Percy p. 329); at Eisenerz first dry then wet "Stuebbe" (charcoal fines) strewn on, centre left coal-covered to keep hot, then two men with axes cut it in half and in to the middle, then drive it apart with wedges - "sehr beschwerlich und dauerte zwei Stunden" (Beck I p. 822-823). Percy p. 329: under the hammer, gently, into a round cake 3-4 in thick, cut into two near-equal parts, drawn into bars; "Eight men were required for the operation of working up the lump by hammering, cutting, etc." Overman: flattened by a tilt hammer into 4-inch slabs, cut into blooms and stretched into bar (p. 142). Elsewhere lumps of 6-7 Ztr were pulled out by hand with hooks and tongs and put under the water hammer, hewn with a set into pieces ("Kotlizhe") (Beck I p. 822).

B10. Repair between heats (Eisenerz)

  • Percy p. 329: "This preparation consisted in cleaning out and repairing the hearth, and covering the bottom with a level and solid brasque of moistened charcoal powder." Beck I p. 823: while two men cut the lump, two others repair the oven: throw in charcoal fines, pour water, level and beat the hearth bottom smooth; take a pre-formed clay brick and bore the tuyere with a pointed iron (see B4). "Anderer Formen bediente man sich bei den Stuckoefen nicht."
  • The tuyere and the breast bricks therefore are rebuilt every heat; the stack walls stand across heats (12 years by Swedenborg's account, OCR); the hearth stone wears (Schmalkalden, B3).
  • Percy p. 328: in some places the slag tap was first made lower and raised, with the tuyere, as the metallic mass at the bottom grew.

B11. Products, yield, fuel, losses

  • Eisenerz, one heat: lump 13-14 quintals plus 6-7 quintals of iron that "flowed out of the furnace, and which, therefore, were steel or cast-iron" = 20 in all (Percy p. 329; Beck I p. 823 "circa 20 Ztr Eisen, in allen drei Modifikationen"). Schmalkalden: lump 4-6 cwt from 216-234 cubic feet of charcoal (Percy p. 329).
  • Quality: Percy p. 329 (Quantz): "soft, tough, and malleable, though less so than bar-iron; he considered it as intermediate between cast and bar-iron." Overman p. 141: the iron "has always been of a superior kind, favorable for the manufacture of steel"; the lump "consists of a mixture of iron and steel"; the blooms "a mixture of fibrous iron, steel, and cast iron", the cast part running into the forge fire. Percy p. 326: "the metallic lump is occasionally carburized to such a degree that it must be subjected to a decarburizing process" and cast iron was nearly always made "to the annoyance of the smelter" (p. 320).
  • Beck I p. 823: the pig ("Graglach") put with the cut lump into the "Loeschherd" (quenching hearth), the origin of the finery; slag contained about 30 % iron; wash-iron recovered by stamping and washing.
  • Yield: Swedenborg, Eisenerz (Beck II p. 172, OCR): "aus 1 Zentner Erz 39 1/2 Pfund Rauheisen" and for 1 Zentner of iron 2 Fass (=10 Wiener Scheffel) of charcoal. INFERRED from Beck I p. 822-823: 13 tubs x 3.5 Ztr = about 45 Ztr of ore for about 20 Ztr of metal, about 44 %.
  • Fuel: Beck I p. 823 charcoal "betraechtlicher als bei den Flossoefen"; Karsten gave consumption of fuel as the reason the type died (Percy p. 326). 1745 Vordernberg 5.05 Fass per Ztr = 36.5 cubic feet "nearly as much as is now used" for smelting plus refining (Beck I p. 823).
  • Switching: at Henneberg the same furnace made pig or Stueck by setting the tuyere back so it no longer projected into the furnace - "So unmittelbar ging der Stuckofenbetrieb in den Hochofenbetrieb ueber" (Beck I p. 824); Percy p. 329 the furnaces that replaced them were called Blauofen, "no essential difference" between them at first.

B12. Crew

  • Schmalkalden: 3 men at a time in 8-hour shifts, 6 days (Percy p. 329). Eisenerz: 2 men cutting the lump, 2 repairing the oven (Beck I p. 823), plus smelter and helpers on the heat (not counted); 8 men for hammering and cutting at Schmalkalden (Percy p. 329).

B13. What goes wrong

  • The mass fuses and sticks to the hearth (Percy p. 328). Slag not tapped: the iron cools and cannot be detached, and the furnace is damaged (Percy p. 328).
  • Too much carburisation: pig iron forms with the Stueck, "Graglach", from the height of the shaft (Beck I p. 823); at Henneberg raising the charge or setting the tuyere back makes pig.
  • Hearth wear changes yield and charcoal use (Percy p. 327). Bellows and tuyere wet and dark all heat (Beck I p. 825). The Styrian smelters held that their ore "would not bear" a continuous even heat and needed the interrupted working; Beck calls it superstition (Beck I p. 819).

C. Not given by the sources read

  • Air furnace: no inside size in metric or any heat time; no fuel quantity per melt; no temperature (Ure says only that bell-metal is far more fusible than copper; Denison "small bits will melt in a common house fire"); no crew count; no number of tapholes beyond one; Biringuccio's drawing of the hearth is lost in the OCR (the plan text is read from garbled lines, car. 102); the braccio is not defined in the text read; Diderot and Smith and Gnudi not read.
  • Stueckofen: no temperatures; no flux; no figure for the shaft refractory except the Swedenborg 12-year account (OCR); no description of the hearth brasque thickness; no bellows count or size for the Styrian type (Overman gives "at least two", Percy and Beck one tuyere); no ore size (Agricola's "nut size", Beck I p. 818, is for a "taller furnace" of doubtful type); the Jars original not read.
  • Dates for the air furnace itself: Biringuccio 1540 only; the type's invention is not dated in the sources read.

D. Summary table

FurnaceInside sizeDraught / blastChargeHeat lengthProductsPage
Founder's air furnace (Biringuccio, 1540)hearth about 2.5 braccia (1.45 m) across, 3.5 to 3.67 braccia (2.0-2.1 m) long, plan "like a lute"; roof about 1.25 braccia (0.7 m) over the floor; walls 0.75-1 braccia; fire trench as long as the furnace, half a braccio under the entry floor (INFERRED metric)chimney draught only: fire at one end on a sloped grate, bridge, two flame windows, two small chimneys; no bellowscopper-tin alloy (12-25 % tin) in pigs on brick bits, scrap after, tin last; no weight given; several furnaces for a very large castnot given (long careful heat; a stuck charge "a month of fire" will not melt); pour when sample "liquid as water or oil"molten bronze tapped by iron pin and plug through a brick channel (a quarter braccio square) to a pit mould: cannon upright, bells mouth-downVII ch. 1-7, car. 101-111; VI ch. 10-14, car. 89-99
Air furnace as 19th century bell-founding trough (Denison, Ure)long shallow trough, bridge or low roof; elliptical for bronze, dome-top for bellschimney at the far end; wood (Whitechapel) or coal/coke (Woolwich)bell-metal 3 to 4 Cu : 1 Sn; cannon 90 Cu : 10 Sn; tin lastnot given; Mears's Westminster bell metal sat nine times as long in the furnace as Warner'scast mouth-down in a pitDenison 351-353; Ure 335, 536-538
Welsh copper melting furnace (Percy 1861)dimensions only in figures; sand bed 12-20 incoal fire on bars, large fire-place, fire-bridge, stackore and slag via roof hoppernot given herematte tapped at holePercy 1861, 318-322
Stueckofen, Eisenerz (Jars via Percy and Beck)10-16 ft high; foot about 4 ft x 2.5 ft; belly 4 ft 2 in; throat about 1.5-2 ft; breast 4 ft wide x 2.5 ft high; hearth 4 ft wide x 2.5 ft deepone clay tuyere about 1 ft above the bottom, projecting 2 in, water-wheel bellows on the breast side, removed to draw the lumpspathic ore, aged and roasted, about 45 Ztr (13 tubs) to one lump, charcoal 4 measures to 1 of ore, ore charge increasing; self-fluxing, none added18 h (15 smelt + 3 draw and repair); 7 lumps a week Monday to Saturdaylump 13-14 quintals (about 700 kg) plus 6-7 quintals pig / steel, about 20 in all; slag about 30 % FePercy 326-329; Beck I 816-825
Stueckofen, Schmalkalden (Quantz via Percy)16 ft high (two of 12 ft); bottom 2.5 ft, belly 4 ft 2 in at 8 ft, mouth 1.5 ft; drawing hole 2 ft wideone copper tuyere 14 in above the bottom, 3 in projecting; water-wheel bellowsspathic ore and brown haematite (later finery slag); charcoal 4 : 13 lumps a day, 8 h shifts, no work Sundaylump 4-6 cwt (about 200-300 kg) from 216-234 cu ft charcoalPercy 327-329; Beck I 824-825
Stueckofen (Overman)10-16 ft high, 24 in at bottom and top, about 5 ft at the widest, breast opening about 2 ft squaretwo tuyeres, two bellows on one side (disagrees with Percy/Beck)charcoal and ore, ore after the tuyere deposits ironabout 24 h to a tonsalamander of iron, steel and cast iron, drawn with a swing crane to a tilt hammerOverman 141-142