Overman, The Manufacture of Iron (1851)

Books The Manufacture of Iron

Covers F. Overman, "The Manufacture of Iron, in All Its Various Branches" (1851, 508 pages). Pages below are the book's printed folios, which are the PDF page less six. PDF pages 1-6, 22, 503-505 and 508 carry no text layer (front matter, one contents page, advertisements); the plates were not looked at, and figures are read from the text that describes them. Read by topic, not linearly: ores, their chemistry, assay and mining (pp. 17-79), wood, peat, coal and charcoal burning (pp. 80-118), the theory of fuel (pp. 132-141), the old European furnaces (pp. 141-151), the theory of the blast furnace (pp. 206-242), the Catalan and German forges (pp. 243-256), the theory of refining (pp. 302-333), fire brick, motive power, the German, blister and Damascus steels (pp. 465-475) and the appendix tables were skipped; rails and sheet were skimmed.

What the book says

Roasting (pp. 39-48, 172, 446)

  • Every ore but the red impalpable oxide should be roasted. Magnetic ore melts to a slag at a cherry red, so the heat is kept low (p. 39). Ore is broken to 2-3 in. first (p. 40).
  • Three methods: kilns, mounds and heaps (p. 40). The shaft kiln is built like a limekiln, 12-18 ft high, holding 50-100 t, worked without stopping on alternate beds of coal and ore drawn at the bottom; a 50 t kiln roasts 30 t in 24 h (pp. 41-42). "Reverberatory furnaces have been tried for roasting ores, but with little success; the operation proved too expensive" (p. 43).
  • Heaps are the common method: an 8 in. bed of wood, ore in courses of 18-24 in. with 2 in. of small coal between them, "one inch of fuel to one foot of ore", fired slow and smothered. A row is done in 10-12 days, magnetic ore in six or eight weeks (pp. 44-45).
  • Well roasted ore is red or brown, sticks to the tongue and breaks easily. Ore roasted to a clinker is "as bad as though they were not roasted at all; in fact ... worse" (p. 172). Roasting is "the surest means of saving coal and blast" (p. 172); the book gives no percentage.
  • The furnace's top flame can roast ore (p. 446).

Coking (pp. 119-132)

  • Blast-furnace coke is burnt in heaps or rows in the open; ovens serve cupolas and fineries (pp. 119, 123). A row is about 100 ft by 7-8 ft by 3 ft (p. 121), and is done "when the white flames of carburetted hydrogen cease to be visible", then covered (p. 122).
  • The Pittsburgh oven (pp. 123-125): a 10 by 10 ft hearth, 2 ft doors bricked up with draught holes, a 20-24 in. hole in the crown, 75-80 bushels laid 12 in. deep. Coking takes 10-12 h, then the top is closed and the oven cools 8-10 h. "After the first and second heats, it needs no kindling"; the first heat is raw at the bottom and spongy at the top, and "the hotter the oven, the better the coke". The coke is drawn hot with bars and scrapers.
  • English ovens are 10 by 12 ft and take 2-3 t (p. 126); the Silesian oven takes two charges a week and saves the tar (p. 128).
  • Good coke is silvery and rings like crockery (p. 129). Quenching with water is "a bad habit; it injures the coke, makes it rotten" (p. 130). 75 % by weight is a good English yield, and ovens give twelve per cent more than heaps (pp. 130-132).

The blast furnace: building and starting (pp. 152-175, 182)

  • A charcoal stack is 35 ft, the hearth 5 ft 6 in. high, two tuyeres (pp. 152-154). The trunnel head is a 10-12 ft chimney with an iron charging door shut after every charge (pp. 157-158).
  • A new stack is dried by seven weeks of firing, eight or ten in a cold season (p. 164). It starts on half burden with gentle blast; 9-10 t in the first week, 16-18 t a week after (p. 165). The coal charge is constant and the ore varied (pp. 165, 194-195).
  • The first cast comes on the second or third day. A cold bottom makes chilled iron, and cold cinder built up above the tuyeres compels "a scraping of the materials out of the furnace" (p. 173). Fuel per ton "chiefly depends upon the composition of the cinders or slag" (p. 173).
  • Blast: soft charcoal bears only 1/2-5/8 psi, strong charcoal 3/4-1 psi; a weak blast burns more coal and makes white metal. The air should be dry (p. 170). "A narrow top, high stack, soft coal" want more volume at weak pressure; "a wide throat, low stack, hard coal" want stronger pressure and less volume (p. 171). Coke furnaces run 40-50 ft with heavier blast (p. 175).
  • Phoenixville anthracite furnace No. 1, per ton of iron: 2.59 t ore, 1.83 t coal, 1.14 t lime (p. 182).

Running the furnace (pp. 184-206)

  • Charges start small, with flux equal to an ore charge at the start (p. 185). Half pressure for the first days, full after a week, full make in 3-4 weeks (p. 186).
  • Cinder is drawn every 12 h at charcoal furnaces, every 6 h at coke furnaces, every 2 h if the hearth is chilling (p. 186). A cold hearth is recovered with "dead charges", charges without ore, six to twelve or more (p. 187).
  • "The tuyere should be bright and star-like." A cold cinder nose forming around it makes "the dark or black tuyere" (pp. 187-188). A cold hearth shows black or dark green cinder and tuyeres working dark (p. 190); the ringer bar clears the hearth from the dam to the back (pp. 189-190).
  • Filling is kept regular: charges by measure and weight, barrows and boxes, a suspension railroad and a water-balance hoist (pp. 191-195). Ores are premixed before weighing on a yard bed, with the flux spread over the top (the Moellerung, pp. 199-200), not stacked in layers inside the furnace. Filling one side only causes scaffolding (p. 200).
  • Casts at six and six; iron left long in the hearth turns white (p. 201). A light burden makes gray iron, a heavy one white, and mottled is the profitable middle (p. 202).
  • Too much lime: the slag blazes and turns spongy like pumice when sprinkled. Too little: "a dark, black, or green" cinder, balls, a blackened tuyere, sticking to the hearthstones (p. 203). Glassy greenish cinder is sound; brown streaks mean less ore within hours or black cinder within 24 h (pp. 203-204).
  • The top flame (pp. 204-205): "a heavy, dark top flame indicates that the furnace is cold, and that the burden is too heavy"; "a bright smoky flame, which throws off white fumes" means too liquid a cinder, too much lime, too light a burden; "an almost invisible, lively flame at the top is significant of a healthy state"; "where the flame wavers, that is, where it is sometimes large and sometimes small, there is, without doubt, scaffolding". The timp flame reads by the same rules.
  • Gray metal runs very liquid and stays so; white metal chills fast with a rough, concave face (p. 205). The pig-bed sand is dug and wetted after each cast (p. 206).

Blowing and hot blast (pp. 394-442)

  • Wooden cylinder bellows (pp. 395-396): two round tubs with pistons worked from below by a beam and crank, and a dry receiver on top whose piston carries "a box filled with iron or stones, to counterbalance the pressure". "From eight to ten strokes" a minute supply a charcoal furnace; tubs and receiver 4-4.5 ft wide and 4 ft high, a 3 ft stroke.
  • A crank gives an irregular blast, which the receiver evens (pp. 410-413). Pipes run 10 in. per 1000 cu ft a minute (p. 414); the nozzle sets the pressure (p. 416).
  • "In wooden cylinders, a pressure as high as five-eighths or three-quarters" psi is the limit; "anthracite, coke, and hard charcoal furnaces cannot be carried on to advantage without iron bellows" (p. 426). "Pressure is an equivalent for hot blast" (p. 427).
  • Hot blast saves thirty to sixty per cent of fuel in anthracite and coke furnaces and nearly doubles the make; hard charcoal saves twenty per cent and makes fifty per cent more; soft charcoal gains little (p. 442). The waste gas is drawn 3-4 ft below the top to boilers and the stove (pp. 444-451).

Puddling (pp. 256-302)

  • The finery that preceded it is described and judged costly (pp. 256-259).
  • The puddling furnace: a 30-40 ft stack with a damper worked by a wire, a 22 by 27 in. door on a chain and lever with a work hole in it, a hearth 5-6 by 3.5-4 ft on air-cooled cast-iron plates, a new furnace dried 3-4 days, a bottom of pounded cinder melted in (pp. 261-266).
  • The heat (pp. 266-268): red in 15 min, turned, white in 30, under cinder by 45; the damper nearly shut while it is stirred; it "comes to nature" in pea-sized grains; the heat is raised; balls of 12-15 in., 70-80 lb, are made, and the work hole shut for a last heat.
  • Boiling (pp. 268-270): the damper nearly shut, "dark and smoky" with black fumes from the top, blue flames over the mass, the cinder rising from 2 to 10-12 in. like "the boiling of corn". The heat must be high or the balls break under the hammer.
  • After the balls are out, the fused cinder is "let off, through the tap-hole below the work door, into a two-wheeled iron hand-cart" (p. 270). At Hyanges the main body of cinder is tapped mid-heat (pp. 275-276).
  • Pittsburgh: 350 lb a charge, six heats (puddlers) or five (boilers) a turn (pp. 270-271). The double furnace takes 700-900 lb through two doors (pp. 273-275).
  • Loss: "four or five per cent" on good white metal, twenty and more on bad; gray pig worked with ore yields ninety-five to ninety-eight per cent (pp. 301-302).

Shingling and forging (pp. 334-344)

  • Tilt and helve hammers of 50-400 lb; 300-400 lb for 60-100 lb blooms (p. 334). A hammer for drawing iron wants at least 150 strokes a minute; the steam hammer gives 80-100 and so shingles rather than draws (pp. 336-337, 339).
  • The steam hammer's anvil has a raised 1 in. shingling face across it and a drawing face at right angles (p. 340). It "crumbles those balls which have been carelessly put together" (p. 341).
  • Squeezers: the lever squeezer at 80-90 strokes a minute, Burden's rotary squeezer in seconds a bloom (pp. 341-344). Balls sent straight to the rolls, as in Europe, leave unsound ends (p. 344).

Rolling, reheating and shearing (pp. 344-388)

  • Roughing grooves reduce "in the proportion of the squares of eleven to fifteen, or nearly one-half"; the first takes a 6 in. bloom (p. 347). Rough rolls turn 30-40 rpm (p. 349); merchant rolls run 7-8 ft a second at the surface (p. 358).
  • "The loss at the roughing rollers, caused by the iron getting too cold, is, of all others, the most disagreeable, because the iron is generally too long to be re-heated, and too thick to be cut" (p. 360).
  • The reheating furnace: a sand hearth sloped to the flue, cinder running out at the end (pp. 371-372). "Work slowly from the commencement", hold below a welding heat, then raise it suddenly and "draw as fast as the rollers will receive" (p. 373). Iron "too long exposed to the influence of the flame in the re-heating furnace" loses its carbon, strength and lustre (p. 384). Piles put the weakest iron in the middle and the best outside (pp. 386-388).
  • The shear: a cast lever on an eccentric or a crank, the upper cutter at an angle to the lower "seldom greater than fifteen degrees"; bar over 2 in. square is sawn (pp. 378-381).

Cast steel (pp. 475-477)

  • 50 lb crucibles in a small air furnace, 1-3 h a melt; "a sudden charge of cold fuel is apt to crack the crucible" (p. 477).